Polyamide resin composition and molded article
By using a specific proportion of copper compounds, glass fibers and halides in the polyamide resin, combined with colorants, the problem of color change caused by moisture in the polyamide resin composition is solved, the mechanical properties and heat aging resistance are maintained, and the Stability of hue.
Patent Information
- Application Number
- CN202380022320.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-18
- Filing Date
- 2023-02-15
- Publication Date
- 2024-09-27
AI Technical Summary
When existing polyamide resin compositions contain copper compounds, color changes due to water absorption, making it difficult to maintain mechanical properties and heat aging resistance while suppressing discoloration caused by moisture.
By combining specific amounts of polyamide resin, copper compounds and glass fibers with low boron content, a polyamide resin composition is prepared, combined with an alkali metal or alkaline earth metal halide and a colorant, to control the mole content of the composition Ratio of elements to fiberglass to suppress color change due to moisture.
It is achieved that the discoloration caused by moisture is effectively suppressed without reducing the mechanical properties and heat aging resistance, and the color tone stability of the polyamide resin composition is improved.
Smart Images

Figure BDA0004996878870000351 
Figure BDA0004996878870000421 
Figure BDA0004996878870000461
Abstract
Description
Technical Field
[0001] The present invention relates to a polyamide resin composition and a molded body.
[0002] This application claims priority based on Japanese Patent Application No. 2022-023815 filed in Japan on February 18, 2022, and the contents of which are incorporated herein by reference. Background Art
[0003] Polyamide resins have excellent mechanical properties, thermal properties, and oil resistance. In addition, compared with ordinary polyamide resins without glass fibers, reinforced polyamide resins with glass fibers added to polyamide resins have greatly improved mechanical properties, heat resistance, chemical resistance, etc. Polyamide resins and glass fiber reinforced polyamide resins having such properties are used in various industrial fields.
[0004] As the field utilizing polyamide resin and glass fiber reinforced polyamide resin, materials such as electronic equipment parts and automobile parts can be cited. From the viewpoint of design and reliability, molded products such as electronic equipment parts and automobile parts are required to be thin-walled, miniaturized and lightweight. In addition, these parts are also required to improve mechanical properties. In order to meet this demand, parts made of polyamide resin and reinforced polyamide resin are used to replace parts made of metal in the past, and lightweight and process rationalization are sought.
[0005] In particular, polyamide resins are excellent in heat aging resistance compared to other resins and are therefore suitable as materials for parts in high temperature environments such as the periphery of an engine, a periphery of an electric motor, and a periphery of a battery of an automobile.
[0006] It should be noted that "heat aging resistance" refers to the property of easily maintaining the strength of a molded body of a polyamide resin after it has been exposed to a high heat environment for a long time. When the strength of a molded body after exposure to a high heat environment (molded body after heat aging) is not easily reduced compared to the strength before exposure to high heat, it is evaluated as having excellent heat aging resistance.
[0007] In conventional automobiles with engines, the ambient temperature in the engine compartment is becoming higher and higher as the number of components used in the engine compartment increases and the engine output increases. Therefore, in order to be able to use the polyamide resin in the engine compartment, a polyamide resin that can maintain excellent heat aging resistance for a long time that significantly exceeds the existing level is required.
[0008] In electric vehicles, the areas around the motor and the battery also become high-temperature environments, and thus polyamide resins that can maintain excellent heat aging resistance for a long period of time are also required.
[0009] As a technology for improving the heat aging resistance of polyamide resin, the technology of adding copper compounds (copper oxides, copper salts, organic copper compounds, etc.) and halogen compounds is known. Among the halogen compounds, iodine compounds are generally added, and the technology of combining polyamide resin with copper compounds, iodine compounds and aliphatic carboxylic acid derivatives is known (for example, see Patent Document 1).
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Laid-Open No. 7-18176 Summary of the invention
[0013] Problems to be solved by the invention
[0014] The polyamide resin composition disclosed in Patent Document 1 has improved heat aging resistance by containing a copper compound. However, when a copper compound is contained in a composition as in the polyamide resin composition of Patent Document 1, the composition absorbs moisture in the air, resulting in a problem that the composition tends to change color depending on the water content of the composition, showing a light pink color when the water absorption is small and a light green color when the water absorption is large. Therefore, a new polyamide resin composition with suppressed color change is required.
[0015] The present invention has been made in view of the above circumstances, and its object is to provide a polyamide resin composition capable of suppressing discoloration due to moisture while maintaining mechanical properties and high heat aging resistance. In addition, the present invention also aims to provide a molded body, which uses such a polyamide resin composition as a material and can suppress discoloration due to moisture while maintaining mechanical properties and high heat aging resistance.
[0016] Means used to solve problems
[0017] The present inventors have conducted repeated studies to solve the above problems and have found that a resin composition containing specific amounts of polyamide resin, copper compound and glass fiber containing a specified amount of boron element can solve the above problems, thereby completing the present invention.
[0018] That is, the present invention is as follows.
[0019] [1] A polyamide resin composition, characterized in that the polyamide resin composition contains 100 parts by mass of (A) a polyamide resin, 0.005 parts by mass to 0.3 parts by mass of (B) a copper compound, and 10 parts by mass to 250 parts by mass of (C) glass fibers, wherein the content of boron in the (C) glass fibers is 1% by mass or less relative to the total mass of the (C) glass fibers.
[0020] [2] The polyamide resin composition according to [1] above, wherein the (A) polyamide resin is one or more selected from the group consisting of the following polyamides and the following copolyamides,
[0021] The polyamide is selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I and polyamide MXD6,
[0022] The copolyamide is a copolymer including at least one selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, and polyamide MXD6 as a constituent component.
[0023] [3] The polyamide resin composition according to [1] or [2] above, wherein the (A) polyamide resin comprises (A-1) a main component polyamide and at least one (A-2) different type of polyamide.
[0024] [4] The polyamide resin composition according to [3] above, wherein the molecular weight of the (A-2) different type of polyamide is smaller than the molecular weight of the (A-1) main component polyamide.
[0025] [5] The polyamide resin composition according to [3] or [4], wherein the content of the (A-2) different type of polyamide is 0.01 to 10 parts by mass per 100 parts by mass of the (A) polyamide resin.
[0026] [6] The polyamide resin composition according to any one of [1] to [5] above, characterized in that the polyamide resin composition further contains (D) at least one or both of an alkali metal halide and an alkaline earth metal halide, and the molar ratio of the content of the (D) halogen compound to the content of the (B) copper compound is 2 / 1 to 50 / 1.
[0027] [7] The polyamide resin composition according to any one of [1] to [6] above, wherein the molar ratio (Mg / Si) of the magnesium (Mg) element to the silicon (Si) element in the (C) glass fiber is 0.01 to 0.2.
[0028] [8] The polyamide resin composition according to any one of [1] to [7] above, wherein the content of iron (Fe) in the glass fiber (C) is 0.01% by mass to 2.0% by mass relative to the total mass of the glass fiber (C).
[0029] [9] The polyamide resin composition according to any one of [1] to [8] above, wherein the content of the sodium (Na) element in the (C) glass fiber is 0.1% by mass to 3.0% by mass relative to the total mass of the (C) glass fiber.
[0030]
[10] The polyamide resin composition according to any one of [1] to [9] above, further comprising 0.01 to 5 parts by mass of (E) a colorant based on 100 parts by mass of the polyamide resin composition.
[0031]
[11] The polyamide resin composition according to
[10] above, wherein the (E) colorant comprises at least one selected from the group consisting of titanium oxide, zinc sulfide, zinc oxide, iron oxide, and organic dyes.
[0032]
[12] The polyamide resin composition according to
[11] above, wherein the (E) colorant contains at least one orange colorant.
[0033]
[13] A molded product comprising the polyamide resin composition according to any one of [1] to
[10] above.
[0034]
[14] A molded article, comprising the polyamide resin composition according to
[11] above.
[0035]
[15] A molded product comprising the polyamide resin composition according to
[12] above.
[0036]
[16] The molded article according to any one of
[13] to
[15] above, wherein the molded article is an automobile part.
[0037]
[17] A polyamide resin composition comprising 100 parts by mass of (A) a polyamide resin, 0.005 parts by mass to 0.3 parts by mass of (B) a copper compound, and 10 parts by mass to 60 parts by mass of (C) glass fibers, wherein the tensile strength of the polyamide resin composition after heat aging measured by the following method is 3.0 or more per 1 part by mass of the glass fibers.
[0038] (Tensile strength after heat aging)
[0039] A molded piece of a multipurpose test piece (type A) produced by a method according to ISO 3167 using the polyamide resin composition was heat aged at 200° C. for 1,000 hours in a hot air circulation oven.
[0040] The test piece after heat aging was cooled at 23° C. for 24 hours or more, and then subjected to a tensile test at a tensile speed of 5 mm / min by a method according to ISO527, and the tensile strength (MPa) after heat aging was measured.
[0041] Effects of the Invention
[0042] According to the present invention, a polyamide resin composition can be provided, which can suppress discoloration due to moisture while maintaining mechanical properties and high heat aging resistance. In addition, a molded body can be provided, which uses such a polyamide resin composition as a material, which can suppress discoloration due to moisture while maintaining mechanical properties and high heat aging resistance. DETAILED DESCRIPTION
[0043] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as “the present embodiment”) will be described in detail.
[0044] It should be noted that the following embodiments are examples for explaining the present invention, and the present invention is not limited to the following embodiments, and can be implemented with various modifications within the scope of the gist of the invention.
[0045] 《Polyamide resin》
[0046] The polyamide resin composition of the present embodiment contains (A) polyamide resin (hereinafter sometimes referred to as component (A)), (B) copper compound (hereinafter sometimes referred to as component (B)), and (C) glass fiber (hereinafter sometimes referred to as component (C)). In addition, the polyamide resin composition may contain (D) either or both of an alkali metal halide and an alkaline earth metal halide (hereinafter sometimes referred to as component (D)).
[0047] The mechanical properties, heat aging resistance, and discoloration due to water, which were the subjects of the polyamide resin composition of the present embodiment, were measured and evaluated by the following methods.
[0048] (Preparation of test pieces)
[0049] The polyamide resin composition was pelletized, and a molded piece of a multipurpose test piece (type A) was produced by a method in accordance with ISO3167 using the obtained pellets.
[0050] (Mechanical properties)
[0051] The multipurpose test piece was cut to prepare a test piece of 80 mm×10 mm×4 mm. Next, the prepared test piece was used to perform a bending strength test at a test speed of 2 mm / min in accordance with ISO178 to measure the bending strength (MPa).
[0052] In addition, the prepared test pieces were used to measure the notched Charpy impact strength (kJ / m 2 ).
[0053] (Heat aging resistance)
[0054] The tensile strength before heat aging was measured by conducting a tensile test at a tensile speed of 5 mm / min using a multipurpose test piece according to the method of ISO527.
[0055] In addition, the multi-purpose test piece was heat aged for 1,000 hours at 200° C. in a hot air circulation oven. The multi-purpose test piece after heat aging was cooled at 23° C. for more than 24 hours, and then subjected to a tensile test at a tensile speed of 5 mm / min by a method according to ISO527, and the tensile strength (MPa) after heat aging for 1,000 hours was measured.
[0056] The retention rate of the tensile strength after heat aging relative to the tensile strength before heat aging was determined.
[0057] (Discoloration due to moisture)
[0058] The polyamide resin composition was pelletized, and the obtained pellets were used to produce a flat molded sheet (60 mm×90 mm, thickness 3 mm) by injection molding.
[0059] The flat molded sheet was placed in a constant temperature and humidity room at 23°C and 50% humidity for 50 hours, and L* (brightness), a* (redness), and b* (yellowness) of the center of the molded sheet were measured according to JIS-Z8781.
[0060] Then, the flat molded sheet was dried in a nitrogen atmosphere at 100° C. for 72 hours, and L*, a*, and b* of the center portion of the molded sheet were measured in the same manner as before drying.
[0061] The color difference (ΔE*) of the color tone obtained based on the following formula was defined as the color tone change.
[0062] ΔE*=√{(LS*-LB*) 2 +(aS*-aB*) 2 +(bS*-bB*) 2}
[0063] LS*, aS*, bS*: L*, a*, b* of the molded piece after being placed in a constant temperature and humidity chamber for 50 hours
[0064] LB*, aB*, bB*: L*, a*, b* of the molded sheet after drying in nitrogen atmosphere for 72 hours
[0065] <(A) Polyamide resin>
[0066] In the present specification, "polyamide resin" refers to a polymer compound having a -CO-NH- (amide) bond in the main chain.
[0067] Examples of the component (A) include, but are not limited to, polyamide resins obtained by ring-opening polymerization of lactam, polyamide resins obtained by self-condensation of ω-aminocarboxylic acid, polyamide resins obtained by condensation of diamine and dicarboxylic acid, and copolymers thereof.
[0068] These polyamide resins may be used alone or in the form of a mixture of two or more.
[0069] Hereinafter, the raw materials of the component (A) in the present embodiment will be described.
[0070] Examples of lactams used as monomers of the polyamide resin include, but are not limited to, pyrrolidone, caprolactam, undecanoic acid lactam, and lauryl lactam. These lactams may be used alone or in combination of two or more.
[0071] Examples of the ω-aminocarboxylic acid include, but are not limited to, ω-amino fatty acids which are ring-opening compounds of the lactam obtained by using water. It should be noted that two or more monomers may be used in combination for condensation of the lactam or the ω-aminocarboxylic acid.
[0072] Next, the polyamide resin obtained by condensing a diamine and a dicarboxylic acid will be described.
[0073] First, as diamines used as monomers of polyamide resins, for example, linear aliphatic diamines such as hexamethylenediamine and pentamethylenediamine; branched aliphatic diamines such as 2-methylpentamethylenediamine and 2-ethylhexamethylenediamine; aromatic diamines such as p-phenylenediamine and m-phenylenediamine; alicyclic diamines such as cyclohexanediamine, cyclopentanediamine and cyclooctanediamine, but are not limited thereto.
[0074] On the other hand, examples of dicarboxylic acids used as monomers of polyamide resins include, but are not limited to, aliphatic dicarboxylic acids such as adipic acid, pimelic acid, and sebacic acid; aromatic dicarboxylic acids such as phthalic acid and isophthalic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid.
[0075] The above-mentioned diamine and dicarboxylic acid as monomers may be used alone or in combination of two or more thereof for condensation.
[0076] As the component (A), for example, at least one selected from the group consisting of polyamide and copolymer polyamide can be used, but the present invention is not limited thereto.
[0077] The polyamide is preferably selected from the group consisting of polyamide 4, polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 9T, polyamide 6I and polyamide MXD6, more preferably selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I and polyamide MXD6.
[0078] The copolymer polyamide is preferably a copolymer containing at least one selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, and polyamide MXD6 as a constituent component.
[0079] Among the polyamide resins listed above, as the component (A), a polyamide resin having a melting point of 200° C. or higher is preferred from the viewpoint of improving the heat resistance of the obtained molded article. Preferred components (A) having such characteristics include, for example, one or more selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, polyamide MXD6, and copolymer polyamides containing at least two of these as constituent components, but are not limited thereto.
[0080] In addition, the melting point of (A) component means the melting point calculated|required by the differential scanning calorimetry (DSC method) based on JIS K7121.
[0081] In terms of heat aging resistance, the ratio of carbon atoms to nitrogen atoms (C / N ratio) in the polymer chain of component (A) is preferably greater than 5. More preferably, the C / N ratio is greater than 5 and 15 or less, and even more preferably, greater than 5 and 12 or less.
[0082] Examples of the copolyamide include, but are not limited to, one or more copolymers selected from the group consisting of copolymers of hexamethylene adipamide and hexamethylene terephthalamide; copolymers of hexamethylene adipamide and hexamethylene isophthalamide; and copolymers of hexamethylene terephthalamide and 2-methylpentamethylene terephthalamide.
[0083] In addition, component (A) generally has an amino group or a carboxyl group as a terminal group. The concentration of the amino terminal and the carboxyl terminal contained in component (A) relative to the total amount of component (A) can be determined by using 1 The integrated value of the characteristic signal corresponding to each terminal group in the H-NMR measurement is obtained, and the ratio of their concentrations can be calculated.
[0084] The concentration of the terminal groups of the component (A) can be adjusted by a known method.
[0085] As a method for adjusting the terminal groups, for example, a method using a terminal adjusting agent can be cited, but it is not limited thereto. Specifically, during the polymerization of component (A), one or more selected from the group consisting of monoamines, diamines, monocarboxylic acids and dicarboxylic acids are added in a manner to achieve a predetermined terminal concentration, thereby adjusting the concentration of the terminal groups.
[0086] The timing of adding these components to the polymerization solvent is not particularly limited as long as they fulfill their original function as terminal regulating agents, and an example thereof is a method of adding them when the raw materials of the polyamide resin are added to the polymerization solvent.
[0087] Examples of monoamines used as terminal regulators include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine and naphthylamine; and any mixtures of these monoamines, but are not limited thereto.
[0088] In particular, from the viewpoints of reactivity, boiling point, stability of the blocked terminal, price, and the like, the monoamine is preferably at least one selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline.
[0089] Examples of diamines used as terminal regulators include, but are not limited to, linear aliphatic diamines such as hexamethylenediamine and pentamethylenediamine; branched aliphatic diamines such as 2-methylpentamethylenediamine and 2-ethylhexamethylenediamine; aromatic diamines such as p-phenylenediamine and m-phenylenediamine; and alicyclic diamines such as cyclohexanediamine, cyclopentanediamine, and cyclooctanediamine.
[0090] These diamines may be used alone or in combination of two or more.
[0091] Monocarboxylic acids used as terminal regulators include, for example, aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; and aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthoic acid, β-naphthoic acid, methylnaphthoic acid and phenylacetic acid, but are not limited thereto.
[0092] These monocarboxylic acids may be used alone or in combination of two or more.
[0093] Examples of dicarboxylic acids used as the terminal regulator include, but are not limited to, units derived from aliphatic dicarboxylic acids such as malonic acid, dimethylmalonic acid, succinic acid, glutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, 2,2-dimethylglutaric acid, 3,3-diethylsuccinic acid, azelaic acid, sebacic acid, and suberic acid; alicyclic dicarboxylic acids such as 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as isophthalic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,4-phenylenedioxydiacetic acid, 1,3-phenylenedioxydiacetic acid, biphenyl dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenyl sulfone-4,4'-dicarboxylic acid, and 4,4'-biphenyl dicarboxylic acid.
[0094] These dicarboxylic acids may be used alone or in combination of two or more.
[0095] Relative to 100 parts by mass of polyamide resin composition, from the viewpoint of improving moldability and mechanical strength, the content of component (A) in the polyamide resin composition of the present embodiment is preferably 30 parts by mass to 90 parts by mass, more preferably 30 parts by mass to 80 parts by mass, and further preferably 40 parts by mass to 70 parts by mass. It should be noted that in this specification, when "to" is used to record the numerical range, it refers to the range including the upper and lower limits of the numerical range. If it is the above-mentioned record, "30 parts by mass to 90 parts by mass" refers to "more than 30 parts by mass and less than 90 parts by mass".
[0096] The component (A) in the polyamide resin composition may be a combination of (A-1) a main component polyamide and at least one (A-2) different type of polyamide (different type of polyamide).
[0097] Here, (A-1) main component polyamide refers to a polyamide component that accounts for more than 10 parts by mass in 100 parts by mass of component (A). In addition, (A-2) different type polyamide refers to a polyamide component that accounts for less than 10 parts by mass in 100 parts by mass of component A.
[0098] The ratio of the different types of polyamide (A-2) is preferably 0.01% to 10% by mass, more preferably 0.05% to 8% by mass, further preferably 0.1% to 7% by mass, and most preferably 0.5% to 5% by mass in 100 parts by mass of the component (A). When the ratio of the different types of polyamide (A-2) in the component (A) is below the upper limit, there is a tendency to improve the retention rate of the Charpy impact strength and the heat aging resistance in a balanced manner. In addition, when the amount of the different types of polyamide (A-2) in the component (A) is above the lower limit, there is a tendency to further improve the retention rate of the heat aging resistance.
[0099] For example, the component (A) may be a mixture of two (A-1) main component polyamides and two (A-2) different types of polyamides.
[0100] As the constituent component of the polymer of different polyamides (A-2), similar to the above-mentioned polyamides and copolyamides constituting the component (A), at least one selected from the group consisting of the following polyamides and copolyamides can be mentioned.
[0101] Polyamide: at least one selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, and polyamide MXD6.
[0102] Copolyamide: A copolymer containing at least one selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, and polyamide MXD6 as a constituent component.
[0103] Among them, from the viewpoint of appearance and color tone change of the polyamide resin composition and its molded article, polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, and polyamide 6I are preferred, polyamide 6, polyamide 66, polyamide 610, polyamide 612, and polyamide 6I are more preferred, and polyamide 6, polyamide 66, and polyamide 6I are further preferred.
[0104] When a polyamide having a molecular weight different from that of the main component polyamide (A-1) is used as the different type polyamide (A-2), the different type polyamide (A-2) preferably has a molecular weight lower than that of the main component polyamide (A-1).
[0105] (A-2) The molecular weight of different types of polyamides was evaluated by the viscosity number measured using 96% by mass sulfuric acid as a solvent according to ISO 307. Specifically, a 0.5% by mass polyamide resin solution was prepared using 96% by mass sulfuric acid as a solvent at 25°C, and the viscosity number of the solution was measured and evaluated.
[0106] (A-2) The viscosity number (VN) of the different types of polyamide is 70 mg / mL to 150 mg / mL, preferably 80 mg / mL to 150 mg / mL, more preferably 100 mg / mL to 150 mg / mL, and further preferably 120 mg / mL to 145 mg / mL.
[0107] When the viscosity number is within the above range, a polyamide resin composition having excellent fluidity during injection molding and excellent mechanical strength and appearance when formed into a molded product can be provided.
[0108] [(B) Copper compounds]
[0109] As component (B), for example, copper halide, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, etc.; or copper complex salts formed by coordination with chelating agents such as ethylenediamine and ethylenediaminetetraacetic acid, etc., but not limited thereto. These copper compounds can be used alone or in combination of two or more. Among them, from the viewpoint of suppressing molecular weight reduction and heat aging resistance during melt mixing, cuprous iodide, cuprous bromide, cupric bromide, cuprous chloride, and cupric acetate are preferred, and cuprous iodide is more preferred.
[0110] The content of the component (B) is preferably 0.005 to 0.3 parts by mass, more preferably 0.0130 to 0.2 parts by mass, and even more preferably 0.05 to 0.15 parts by mass, relative to 100 parts by mass of the component (A), in terms of the copper element in the copper compound. When the concentration of the copper element is within the above range relative to 100 parts by mass of the component (A), the heat aging resistance of the polyamide resin composition is further improved and the precipitation of copper and the tendency of metal corrosion can be effectively suppressed.
[0111] [(C) Glass fiber]
[0112] The cross section of the component (C) (glass fiber) may be circular or flat (elliptical, cocoon-shaped, etc.), but is preferably flat from the viewpoint of low warpage.
[0113] When the cross section of the component (C) is circular, the number average fiber diameter of the component (C) is preferably 3 μm to 30 μm, more preferably 9 μm to 20 μm, and further preferably 12 μm to 19 μm, from the viewpoint of mechanical strength and appearance.
[0114] When the cross section of the component (C) is flat, the average minor diameter of the glass fiber is preferably 3 μm to 15 μm, more preferably 4 μm to 10 μm, and even more preferably 5 μm to 9 μm from the viewpoint of mechanical strength, appearance, and low warpage.
[0115] Regardless of whether the cross section of the component (C) is circular or flat, the average cross-sectional area of the component (C) is preferably 50 μm from the viewpoint of excellent mechanical strength and appearance. 2 Above and 350μm 2 Below, more preferably 100 μm 2 Above and 300μm 2 Below, more preferably 120 μm 2 Above and 250μm 2 The average cross-sectional area is a value obtained by photographing a cross section of the (C) glass fiber using a microscope, measuring the cross-sectional areas of 50 randomly selected fibers, and averaging the measured values.
[0116] The content of the boron element in the component (C) is 1% by mass or less, more preferably 0.5% by mass or less, based on the total mass of the component (C), and it is further preferred that the boron element is not contained.
[0117] When the content of the boron element in the component (C) is within the above range, the mechanical strength, rigidity, dimensional accuracy and appearance of a molded article obtained from the polyamide resin composition tend to be more excellent.
[0118] In the component (C), the ratio (Mg / Si) of the magnesium (Mg) element to the silicon (Si) element contained in the component (C) is preferably 0.01 to 0.2, more preferably 0.01 to 0.1, further preferably 0.01 to 0.05, and further preferably 0.01 to 0.025. Alternatively, the ratio (Mg / Si) of the magnesium (Mg) element to the silicon (Si) element contained in the component (C) is preferably 0 to 0.025.
[0119] When the Mg / Si ratio is within the above range, the change in color tone of the molded article due to water absorption can be further suppressed, and a polyamide resin composition having a more excellent color tone change tends to be obtained.
[0120] In the (C) component, the content of iron (Fe) element is preferably 0.01 mass % to 2.0 mass %, more preferably 0.05 mass % to 1.0 mass %, further preferably 0.1 mass % to 0.75 mass %, further preferably 0.15 mass % to 0.7 mass %, and most preferably 0.2 mass % to 0.6 mass %, relative to the total mass of the (C) glass fiber.
[0121] When the content of the iron element in the component (C) is within the above range, the change in color tone of the molded article due to water absorption can be further suppressed, and a polyamide resin composition having a more excellent color tone change tends to be obtained.
[0122] In the (C) component, the content of sodium (Na) element as an alkali ion is preferably 0.1 mass % to 3.0 mass % relative to the total mass of the (C) glass fiber, more preferably 0.1 mass % to 2.0 mass %, further preferably 0.3 mass % to 1.8 mass %, further preferably 0.4 mass % to 1.7 mass % and most preferably 0.5 mass % to 1.6 mass %.
[0123] When the sodium element content in the component (C) is within the above range, the mechanical strength, rigidity, dimensional accuracy and appearance of a molded product obtained from the polyamide resin composition tend to be more excellent.
[0124] The content of component (C) in the polyamide resin composition is preferably 10 to 250 parts by mass, more preferably 15 to 150 parts by mass, and further preferably 15 to 125 parts by mass, relative to 100 parts by mass of the polyamide resin. Alternatively, the content of component (C) in the polyamide resin composition is preferably 10 to 60 parts by mass, relative to 100 parts by mass of the polyamide resin.
[0125] When the content of the component (C) is within the above range, the mechanical strength, rigidity, dimensional accuracy and color tone of a molded product obtained from the polyamide resin composition can be further improved.
[0126] The component (C) contains at least one of a surface treatment agent and a sizing agent. For example, at least one of a surface treatment agent and a sizing agent may be applied to the glass fiber. When the component (C) contains at least one of a surface treatment agent and a sizing agent, the processability, especially the defibration property, is further improved.
[0127] There are no particular restrictions on the surface treatment agent of component (C), and for example, a silane coupling agent is suitable. There are no particular restrictions on the above-mentioned silane coupling agent, and examples thereof include: aminosilanes such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; epoxysilanes; and vinylsilanes. Among them, aminosilanes are preferred. It should be noted that the surface treatment agent can be used alone or in combination of two or more.
[0128] The sizing agent of the component (C) is not particularly limited, and examples thereof include the following (a) to (f):
[0129] (a) Epoxy resin (sizing agent (a))
[0130] (b) Polyurethane resin (sizing agent (b))
[0131] (c) Homopolymer of acrylic acid (sizing agent (c))
[0132] (d) Copolymers of acrylic acid and other copolymerizable monomers (sizing agent (d))
[0133] (e) Salts of the above homopolymers or copolymers with primary, secondary or tertiary amines (sizing agents (e))
[0134] (f) A copolymer comprising an unsaturated vinyl monomer and an unsaturated vinyl monomer containing a carboxylic anhydride as structural units (sizing agent (f))
[0135] It should be noted that the unsaturated vinyl monomer in the sizing agent (f) does not include a carboxylic anhydride-containing unsaturated vinyl monomer.
[0136] These sizing agents may be used alone or in combination of two or more.
[0137] Among them, the sizing agent as component (C) is preferably sizing agent (a), (b), (f) or a combination thereof, and more preferably sizing agent (b), (f) or a combination thereof. The use of such a sizing agent tends to further improve the mechanical strength of the resin composition.
[0138] The carboxylic anhydride-containing unsaturated vinyl monomer constituting the sizing agent (f) is not particularly limited, and examples thereof include maleic anhydride, itaconic anhydride, citraconic anhydride, etc. Among them, maleic anhydride is preferred.
[0139] The unsaturated vinyl monomer constituting the sizing agent (f) is not particularly limited, and examples thereof include styrene, α-methylstyrene, ethylene, propylene, butadiene, isoprene, chloroprene, 2,3-dichloroprene, 1,3-pentadiene, cyclooctadiene, methyl methacrylate, methyl acrylate, ethyl acrylate, ethyl methacrylate, etc. Among them, styrene or butadiene is preferred.
[0140] Preferred sizing agents (f) are not particularly limited, and examples thereof include copolymers of maleic anhydride and butadiene, copolymers of maleic anhydride and ethylene, copolymers of maleic anhydride and styrene, and mixtures thereof.
[0141] In addition, the lower limit of the weight average molecular weight of the sizing agent (f) is preferably 2,000, and more preferably 5,000. In addition, the upper limit of the weight average molecular weight of the sizing agent (f) is preferably 1,000,000, and more preferably 500,000. When the weight average molecular weight of the sizing agent (f) is within the above range, the fluidity of the polyamide resin composition tends to be further improved. It should be noted that the weight average molecular weight in this specification can be measured by gel permeation chromatography (GPC).
[0142] As the sizing agent (a), there is no particular limitation, for example, it is preferred to use an epoxy resin having at least two glycidyl groups, wherein an epoxy resin obtained by reacting bisphenol with epihalohydrin is more preferred. The molar equivalent of the epoxy group in the sizing agent (a) is preferably 180 g / mol equivalent or more, more preferably 450 g / mol equivalent or more and 1900 g / mol equivalent or less. By having the epoxy equivalent within the above range, there is a tendency that the bundling property of the glass fiber (B) is further improved.
[0143] The sizing agent (b) is not particularly limited as long as it is a polyurethane resin generally used as a sizing agent for the component (C), and examples thereof include polyurethane resins synthesized from isocyanates such as meta-xylylene diisocyanate (XDI), 4,4'-methylenebis(cyclohexyl isocyanate) (HMDI) and isophorone diisocyanate (IPDI) and polyester or polyether diols.
[0144] The weight average molecular weight of the sizing agent (c) is preferably 1,000 to 90,000, more preferably 1,000 to 25,000, and even more preferably 1,000 to 25,000. The weight average molecular weight can be measured by a conventional method using GPC.
[0145] The copolymerizable monomers constituting the sizing agent (d) are not particularly limited, and examples thereof include monomers having at least one of a hydroxyl group and a carboxyl group. Such monomers having at least one of a hydroxyl group and a carboxyl group are not particularly limited, and examples thereof include at least one selected from the group consisting of acrylic acid, maleic acid, methacrylic acid, vinyl acetate, crotonic acid, isocrotonic acid, fumaric acid, itaconic acid, citraconic acid, and mesaconic acid (except for the case of only acrylic acid). Among the above monomers, it is preferred to have at least one ester monomer.
[0146] The primary amine, secondary amine or tertiary amine constituting the sizing agent (e) is not particularly limited, and examples thereof include triethylamine, triethanolamine, glycine, etc. From the viewpoint of improving the stability of a mixed solution with other chemical reagents (such as a silane coupling agent) and reducing amine odor, the degree of neutralization is preferably 20% by mass or more and 90% by mass or less, more preferably 30% by mass or more and 80% by mass or less, and even more preferably 40% by mass or more and 60% by mass or less.
[0147] The weight average molecular weight of the acrylic polymer constituting the sizing agent (e) is not particularly limited, but is preferably in the range of 3,000 to 50,000. When the weight average molecular weight is above the above lower limit, the bundling property of the glass fiber tends to be further improved. In addition, when the weight average molecular weight is below the above upper limit, the mechanical properties of the resin composition tend to be further improved.
[0148] When treating component (C) with at least one of a surface treatment agent and a sizing agent, a lubricant is preferably used. The lubricant is not particularly limited, and for example, any conventional liquid or solid lubricant material can be appropriately used according to the purpose. Such a lubricant is not particularly limited, and examples thereof include: animal, plant, or mineral waxes such as carnauba wax and lanolin wax; fatty acid amides, fatty acid esters, or fatty acid ethers; surfactants such as aromatic esters or aromatic ethers.
[0149] ((C) Method for producing glass fiber)
[0150] The component (C) is obtained by coating (applying) at least one of the surface treatment agent and the sizing agent on the glass fiber using a known method such as a roll coater in a known glass fiber production process, and drying the produced fiber bundle to continuously react.
[0151] It should be noted that the state of the component (C) is not particularly limited, and for example, the glass fiber bundle can be used directly in the form of roving, or can be used in the form of chopped strands after further cutting. It should be noted that the fiber bundle can be dried after the cutting process or before the cutting process.
[0152] The amount of at least any one of the surface treatment agent and the sizing agent deposited is preferably 0.2% by mass to 3% by mass, more preferably 0.2% by mass to 2% by mass, and even more preferably 0.3% by mass to 2% by mass, based on solid fraction, relative to 100% by mass of the component (C).
[0153] When the amount of at least one of the surface treatment agent and the sizing agent attached is greater than the above lower limit, the bundling property of the glass fiber tends to be further improved. On the other hand, when the amount of at least one of the surface treatment agent and the sizing agent attached is less than the above upper limit, the thermal stability of the resin composition tends to be further improved.
[0154] The component (C) may be used alone or in combination of two or more components that differ in cross-sectional shape, average cross-sectional area, glass composition, surface treatment agent, sizing agent, etc.
[0155] The component (C) may be used in the form of roving, or may be used in the form of chopped strands cut into a length of about 2 mm to about 5 mm.
[0156] The weight average fiber length of the component (C) is preferably 100 μm to 800 μm, more preferably 200 μm to 700 μm, and even more preferably 300 μm to 650 μm, from the viewpoint of mechanical strength and appearance.
[0157] The weight average fiber length of component (C) can be measured, for example, by the following method: heating incineration pellets at a temperature above the decomposition temperature of the polyamide resin composition, taking a photo of the residual ash using a microscope, and measuring the glass fiber length. As a method for calculating the weight average fiber length based on the measured value obtained using a microscope, the following formula can be cited.
[0158] [Weight average fiber length] = [Sum of squares of glass fiber lengths] / [Sum of glass fiber lengths]
[0159] [(D) Alkali metal halide and / or alkaline earth metal halide]
[0160] As component (D), there is no particular limitation, and examples thereof include: potassium iodide, potassium bromide, potassium chloride, sodium iodide, sodium chloride, calcium iodide, calcium bromide and calcium chloride, and mixtures thereof. Among them, as component (D), preferably potassium iodide and potassium bromide and mixtures thereof, more preferably potassium iodide. By using such a halide, the heat aging resistance of the polyamide resin composition is further improved, and the tendency of metal corrosion can be further suppressed. It should be noted that component (D) can be used alone or in combination of two or more.
[0161] The content of the component (D) in the polyamide resin composition is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 2 parts by mass, and even more preferably 0.05 to 1 part by mass relative to 100 parts by mass of the polyamide resin composition. When the content of the halide is within the above range, the molecular weight reduction and heat aging resistance of the polyamide resin composition are further improved during melt kneading, and the precipitation of copper and the tendency of metal corrosion are further suppressed.
[0162] From the viewpoint of heat aging resistance of the polyamide resin composition, the component (D) is preferably used in combination with the component (B).
[0163] The molar ratio of the content of the component (D) to the content of the component (B) (component (D) / component (B)) is preferably 2 / 1 to 50 / 1. When the molar ratio is within the above range, the decrease in molecular weight during melt kneading can be further suppressed, and a polyamide resin composition with better heat resistance can be obtained.
[0164] When the molar ratio of the component (D) to the component (B) is 2 or more, there is a tendency that copper precipitation and metal corrosion can be further suppressed. On the other hand, when the molar ratio of the component (D) to the component (B) is 50 or less, there is a tendency that corrosion of the screw of the molding machine can be further prevented without almost impairing mechanical properties such as heat resistance and toughness.
[0165] The halogen concentration (molar concentration) [X] in the polyamide resin composition is preferably 40 ppm or more and 9000 ppm or less relative to the component (A).
[0166] When copper halide is used as the component (B), the "halogen" referred to herein means the total of the halogen derived from the copper halide (component (B)) and the halogen derived from the component (D).
[0167] The content of the mixture of the components (B) and (D) in the polyamide resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, further preferably 0.05 to 2 parts by mass, further preferably 0.1 to 1.5 parts by mass, and most preferably 0.5 to 1.3 parts by mass, relative to 100 parts by mass of the polyamide resin composition.
[0168] When the content is within the above range, the heat aging resistance of the polyamide resin composition tends to be further improved.
[0169] [(E) Colorant]
[0170] The polyamide resin composition may contain (E) a coloring agent (hereinafter, sometimes referred to as (E) component).
[0171] As the colorant (E), any one or both of a pigment and an organic dye are preferred. Examples of the pigment include titanium oxide, zinc sulfide, zinc oxide, and iron oxide. That is, the colorant (E) preferably contains at least one selected from the group consisting of titanium oxide, zinc sulfide, zinc oxide, iron oxide, and an organic dye.
[0172] When the polyamide resin composition contains the component (E), the color tone of the component (A) becomes better, thereby improving the appearance of the polyamide resin composition.
[0173] The content of the component (E) in the polyamide resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and still more preferably 0.1 to 1% by mass, relative to 100 parts by mass of the polyamide resin composition. When the content is within the above range, there is a tendency to further improve the moldability of the polyamide resin composition without impairing the mechanical strength of the molded body obtained from the polyamide resin composition.
[0174] The polyamide resin composition may contain an orange colorant having CAS No. 4424-06-0, "CI Pigment Orange 43" (pigment colorant) or CAS No. 6925-69-5, "CI Solvent Orange 60" (dye colorant) as component (E). By coloring the polyamide resin composition in orange, it can be used as a high voltage electrical component material as specified in Regulation No. 100 of the United Nations Economic Commission for Europe (UNECE) "Uniform Provisions on Special Requirements for the Licensing of Electric Drive Vehicles [2015 / 505]". Paragraph 2.17 of the above Regulation No. 100 states: In the classification of motor components or electrical circuits, the term "high voltage" is applied when the effective voltage is greater than 60V and less than or equal to 1500V (DC) or greater than 30V and less than or equal to 1000V (AC) root mean square (rms).
[0175] The “high voltage” classification corresponds to voltage class B of ISO 6469-3:2018 (“Electric Vehicles - Safety Standard - Part 3: Electrical Safety”). Section 5.2 can apply to electrical components of voltage class B indicated by appropriate hazard symbols or “orange”.
[0176] The content of CI Pigment Orange 43 or CI Solvent Orange 60 in the polyamide resin composition is preferably 0.01% to 5% by mass, more preferably 0.03% to 3% by mass, and further preferably 0.1% to 1% by mass, relative to 100% by mass of the polyamide resin composition. When the content of CI Pigment Orange 43 or CI Solvent Orange 60 in the polyamide resin composition is within the above range, there is a tendency that the orange color of the polyamide resin composition can be further improved without impairing the mechanical strength of a molded body obtained from the polyamide resin composition.
[0177] Pigment colorants are preferred because they are more heat resistant than dye colorants and are relatively less likely to fade. For example, from this viewpoint, when comparing CI Pigment Orange 43 and CI Solvent Orange 60, CI Pigment Orange 43, which is a pigment colorant, is less likely to fade and is preferred.
[0178] (Other ingredients)
[0179] The polyamide resin composition may contain other components as necessary in addition to the above-mentioned components (A) to (E) within a range not impairing the effects of the present invention.
[0180] As other components, for example, antioxidants, ultraviolet absorbers, heat stabilizers, light degradation inhibitors, plasticizers, lubricants, release agents, nucleating agents, flame retardants, colorants, dyes, pigments, etc. can be added, and other thermoplastic resins can also be mixed, but are not limited to these.
[0181] Here, since the properties of the other components are greatly different, the appropriate content of each component is various. Moreover, a person skilled in the art can set the appropriate content of each of the other components.
[0182] When the polyamide resin composition contains 100 parts by mass of component (A), 0.005 to 0.3 parts by mass of component (B), and 10 to 60 parts by mass of component (C), the tensile strength after heat aging measured by the following method is preferably 3.0 or more, more preferably 3.0 or more and 5.0 or less per 1 part by mass of glass fiber. When the tensile strength per 1 part by mass of glass fiber is within the above range, heat aging resistance can be imparted to the molded body.
[0183] (Tensile strength after heat aging)
[0184] A molded piece of a multipurpose test piece (type A) produced by a method according to ISO 3167 using the polyamide resin composition was heat aged at 200° C. for 1,000 hours in a hot air circulation oven.
[0185] The test piece after heat aging was cooled at 23° C. for 24 hours or more, and then subjected to a tensile test at a tensile speed of 5 mm / min by a method according to ISO527, and the tensile strength (MPa) after heat aging was measured.
[0186] [Method for producing polyamide resin composition]
[0187] As a method for producing the polyamide resin composition of the present embodiment, for example, a method can be used in which the component (B), the component (C), and the component (D) as required are kneaded in a molten state of the component (A) using a single screw extruder or a multi-screw extruder, but the present invention is not limited thereto.
[0188] More specifically, the following method is preferably used: using a twin-screw extruder having an upstream supply port and a downstream supply port, the (A) component, the (B) component and the (D) component are supplied from the upstream supply port to melt them, and then the (C) glass fiber is supplied from the downstream supply port to melt-knead them. In addition, when using rovings such as glass fiber and carbon fiber, they can be compounded by a known method.
[0189] In addition to the above method, the polyamide resin composition can also be obtained by the following direct addition or by using a polyamide masterbatch.
[0190] Direct addition: adding component (B) and, if necessary, component (D) during the polymerization of component (A), and melt-kneading the resulting polymer and component (C);
[0191] Utilizing a polyamide masterbatch: A method in which a composition (polyamide masterbatch) obtained by melt-kneading a polyamide, the component (B), and, if necessary, the component (D) is further melt-kneaded with the components (A) and (C).
[0192] (Polyamide Masterbatch)
[0193] Examples of polyamides used in the preparation of polyamide masterbatch include, but are not limited to, polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 116, polyamide 11, polyamide 12, nylon TMHT, polyamide 6I, polyamide 9T, polyamide 6T, nylon PACM12, nylon dimethyl PACM12, polyamide MXD6, and polyamide 11T (H).
[0194] Among the above-mentioned polyamides, polyamide 6, polyamide 66, and polyamide 6I are preferred from the viewpoint of compatibility.
[0195] (Organic compound having at least one amide group)
[0196] During the melt kneading for preparing the polyamide masterbatch, an organic compound having at least one amide group (hereinafter sometimes referred to as "amide group-containing organic compound") may be added and mixed. An amide group-containing organic compound refers to a compound having at least one amide group in a molecular chain. Examples of amide group-containing organic compounds include, but are not limited to, monoamides, substituted amides, hydroxymethylamides, and bisamides.
[0197] Monoamides are represented by the general formula R-CONH2 (wherein R is a saturated aliphatic, unsaturated aliphatic, aromatic group having 8 to 30 carbon atoms, or a group in which a part of -H is substituted with -OH). Examples of monoamides used as organic compounds containing amide groups include, but are not limited to, lauryl amide, palmitamide, stearyl amide, behenyl amide, hydroxystearyl amide, oleyl amide, erucyl amide, ricinoleyl amide, and the like.
[0198] Substituted amides are of the general formula R 1 -CONH-R 2 represents (where R 1 and R 2 Each independently represents a saturated aliphatic, unsaturated aliphatic, aromatic group having 8 to 30 carbon atoms, or a group in which a part of -H is substituted with -OH). Examples of substituted amides used as an amide group-containing organic compound include, but are not limited to, N-lauryl lauramide, N-palmityl palmitamide, N-stearyl stearamide, N-oleyl oleamide, N-stearyl oleamide, N-oleyl stearamide, N-stearyl erucamide, N-oleyl palmitamide, N-stearyl 12-hydroxystearamide, and N-oleyl 12-hydroxystearamide.
[0199] Hydroxyl methylamides are represented by the general formula R-CONHCH2OH (wherein R is a saturated aliphatic, unsaturated aliphatic, aromatic group having 8 to 30 carbon atoms, or a group in which a part of -H thereof is substituted with -OH). Examples of the hydroxymethylamides used as the amide group-containing organic compound include, but are not limited to, hydroxymethyl stearamide and hydroxymethyl behenamide.
[0200] Bisamides are represented by the general formula (R-CONH) 2 (CH2) nrepresents (wherein R is a saturated aliphatic, unsaturated aliphatic, aromatic group having 8 to 30 carbon atoms, or a group in which a part of -H thereof is substituted with -OH. In addition, n is 1 to 8). Examples of the bisamides used as the amide group-containing organic compound include, but are not limited to, methylenebislauramide, methylenebislauramide, methylenebishydroxystearamide, ethylenebisoctylamide, ethylenebislauramide, ethylenebisstearamide, ethylenebisisostearamide, ethylenebishydroxystearamide, ethylenebisbehenamide, hexamethylenebisstearamide, hexamethylenebisbehenamide, hexamethylenebishydroxystearamide, butylenebishydroxystearamide, N,N'-distearyl adipamide, N,N'-distearyl sebacamide, methylenebisoleamide, ethylenebisoleamide, ethylenebiserucamide, hexamethylenebisoleamide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacamide, isophthalic acid bisstearamide, and N,N'-distearylisophthalic acid amide.
[0201] The above-mentioned amide group-containing organic compounds may be used alone or in combination of two or more. Among the above-mentioned amide group-containing organic compounds, preferred amide group-containing organic compounds include bisamides from the viewpoint of further improving the dispersibility of copper compounds and halogen compounds.
[0202] The content of the amide group-containing organic compound is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5.0 parts by mass, and even more preferably 1.0 to 4.0 parts by mass, relative to 100 parts by mass of the polyamide constituting the polyamide masterbatch. By setting the content within this range, the dispersibility of the components (B) and (D) constituting the polyamide masterbatch in the polyamide resin is further improved, and the polyamide resin composition and its molded article can be sufficiently improved in heat aging resistance, and copper precipitation and corrosion can be suppressed.
[0203] (Method for producing polyamide masterbatch)
[0204] The polyamide masterbatch is obtained by mixing the above-mentioned component (B), component (D), an amide group-containing organic compound and polyamide.
[0205] The component (B), the component (D) and the amide group-containing organic compound may be added to the polyamide separately, or at least two of these three compounds may be mixed in advance and added to the polyamide. Or at least two of these three compounds may be mixed in advance and crushed and added to the polyamide. Or at least two of these three compounds may be mixed in advance, crushed and made into tablets and then added to the polyamide.
[0206] The component (B), the component (D) and the amide group-containing organic compound may be mixed by a known method, for example, a tumble mixer, a Henschel mixer, a plowshare mixer, a Nauta mixer, a jet mixer or the like.
[0207] A known method can be applied as the method for pulverizing, and for example, any of a hammer mill, a knife mill, a ball mill, a jaw crusher, a cone crusher, a roller mill, a jet mill, a stone mill, etc. may be used.
[0208] The method for forming the tablet can be a known method, for example, any of compression granulation, tableting, dry extrusion granulation, melt extrusion granulation, etc. may be used.
[0209] The content of the polyamide masterbatch in the polyamide resin composition is preferably 0.01 to 5 parts by mass, more preferably 0.3 to 4 parts by mass, and even more preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the component (A).
[0210] [Molded article of polyamide resin composition]
[0211] The molded article of the present embodiment includes the above-mentioned polyamide resin composition and is obtained by, for example, injection molding the polyamide resin composition.
[0212] [use]
[0213] The molded article of the present embodiment can be suitably used as various molded articles or parts for, for example, automobiles, machinery industry, electric and electronic applications, industrial materials, industrial materials, and daily and household products.
[0214] Example
[0215] Hereinafter, the present invention will be described in detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.
[0216] [Evaluation method]
[0217] Hereinafter, the methods of evaluation performed in Examples and Comparative Examples will be described. In each evaluation, pellets of a polyamide resin composition produced in Examples and Comparative Examples described later were used.
[0218] <Viscosity Number (VN)>
[0219] The viscosity number was measured using the produced pellets in accordance with ISO 307 (JIS-K6933). More specifically, the viscosity number was measured at 25°C using a polyamide solution adjusted to 0.5 mass % using sulfuric acid having a concentration of 96% as a solvent.
[0220] <Weight Average Fiber Length of Glass Fiber>
[0221] The produced pellets were heated in an electric furnace at 650° C. for 2 hours and incinerated. 500 glass fibers were randomly selected from the residue component, and the fiber length was measured using a SEM photograph at a magnification of 1000. Next, the weight average fiber length was calculated using the following formula.
[0222] [Weight average fiber length] = [Sum of squares of glass fiber lengths] / [Sum of glass fiber lengths]
[0223] <Test piece preparation: Multi-purpose test piece (Type A) molding piece>
[0224] A multi-purpose test piece (type A) was produced from the produced pellets by a method in accordance with ISO3167 using an injection molding machine (PS-40E, manufactured by Nissei Plastic Industry Co., Ltd.).
[0225] At this time, the following settings were made: injection and holding time was 25 seconds, cooling time was 15 seconds, mold temperature was 80°C, and molten resin temperature was 290°C.
[0226] <Preparation of test piece: flat plate molded piece>
[0227] A flat molded sheet was manufactured from the manufactured pellets as follows: using an injection molding machine (PS-40E, manufactured by Nissei Plastic Industry Co., Ltd.), the cooling time was set to 25 seconds, the screw speed was set to 150 rpm, the mold temperature was set to 80°C, and the barrel temperature was set to 290°C. The injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.0 seconds ± 0.1 seconds, and a flat molded sheet (60 mm × 90 mm, thickness 3 mm) was manufactured from the pellets of the polyamide resin composition.
[0228] <Physical Property Evaluation 1: Tensile Strength>
[0229] Using the multipurpose test piece (Type A), a tensile test was performed at a tensile speed of 5 mm / min by a method in accordance with ISO527, and the tensile strength (MPa) was measured.
[0230] <Physical Property Evaluation 2: Tensile Strength after Heat Aging>
[0231] The multipurpose test piece (type A) was heat aged in a hot air circulation oven at 200° C. for 1,000 hours.
[0232] This was cooled at 23° C. for more than 24 hours, and then subjected to a tensile test at a tensile speed of 5 mm / min by a method according to ISO527, and the tensile strength (MPa) after heat aging for 1,000 hours was measured.
[0233] The retention rate (%) of the tensile strength after heat aging relative to the tensile strength obtained in the above-mentioned <Physical Property Evaluation 1: Tensile Strength> was calculated.
[0234] <Physical Property Evaluation 3: Tensile Strength of Test Specimen after Heat Aging per 1 Part by Mass of Glass Fiber>
[0235] The value obtained by dividing the tensile strength obtained in the above-mentioned <Physical Property Evaluation 2: Tensile Strength after Heat Aging> by the glass fiber ratio (parts by mass) was measured.
[0236] <Physical Property Evaluation 4: Flexural Strength>
[0237] The multipurpose test piece (type A) was cut to prepare a test piece of 80 mm×10 mm×4 mm. Next, the prepared test piece was used to perform a bending strength test at a test speed of 2 mm / min in accordance with ISO178, and the bending strength (MPa) was measured.
[0238] <Physical Property Evaluation 5: Notched Charpy Impact Strength>
[0239] The multi-purpose test piece (type A) was cut to prepare a notched test piece of 80 mm × 10 mm × 4 mm. The notched Charpy impact strength (kJ / m 2 ).
[0240] <Physical Property Evaluation 6: Color Tone Change>
[0241] The flat molded sheet was placed in a constant temperature and humidity room at 23°C and 50% humidity for 50 hours, and the following measurement items were measured at the center of the molded sheet using a colorimeter (ZE-2000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS-Z8781.
[0242] Measurement items: L* (brightness), a* (redness), b* (yellowness)
[0243] Then, the flat molded sheet was dried in a nitrogen atmosphere at 100° C. for 24 hours or 72 hours, and the above-mentioned measurement items were measured at the center of the molded sheet using a colorimetric colorimeter in the same manner as before drying.
[0244] The color difference (ΔE*) of the color tone obtained by using the obtained measurement results according to the following formula was regarded as the color tone change. The smaller the ΔE* of the measured value, the smaller the change of the color tone corresponding to the change of the water content, and the better the identification.
[0245] ΔE*=√{(LS*-LB*) 2 +(aS*-aB*) 2 +(bS*-bB*) 2}
[0246] (LS*, aS*, bS*: L*, a*, b* of the molded piece after being placed in a constant temperature and humidity chamber for 50 hours
[0247] LB*, aB*, bB*: L*, a*, b* of the molded sheet after drying in a nitrogen atmosphere for 24 hours or 72 hours)
[0248] <Physical Property Evaluation 7: Discoloration>
[0249] The flat sheet was placed in a constant temperature and humidity chamber at 80°C and 90% for 300 hours to absorb water. The color difference (ΔE*) from the color tone before the water absorption was taken as the discoloration change. The smaller the color difference ΔE*, the more the discoloration degradation was suppressed.
[0250] [Preparation of raw materials]
[0251] ((A) Ingredients: Main ingredient polyamide and different types of polyamide)
[0252] (PA-1) Polyamide 66
[0253] VN (sulfuric acid): 127 ml / g, amino terminal group: 44 mmol / kg, carboxylic acid terminal group: 75 mmol / kg
[0254] (PA-2) Polyamide 66 / 6I
[0255] VN (sulfuric acid): 117 ml / g, amino terminal group: 47 mmol / kg, carboxylic acid terminal group: 132 mmol / kg
[0256] (PA-3) Polyamide 6I
[0257] VN (sulfuric acid): 62 ml / g, amino terminal group: 58 mmol / kg, carboxylic acid terminal group: 212 mmol / kg
[0258] (PA-4) Polyamide 610
[0259] VN (sulfuric acid): 117 ml / g, amino terminal group: 42 mmol / kg, carboxylic acid terminal group: 65 mmol / kg
[0260] (PA-5) Polyamide 612
[0261] VN (sulfuric acid): 117 ml / g, amino terminal group: 38 mmol / kg, carboxylic acid terminal group: 96 mmol / kg
[0262] (PA-6) Polyamide 6
[0263] VN (sulfuric acid): 112 ml / g, amino terminal group: 41 mmol / kg, carboxylic acid terminal group: 78 mmol / kg
[0264] (PA-7) Polyamide 66
[0265] VN (sulfuric acid): 112 ml / g, amino terminal group: 38 mmol / kg, carboxylic acid terminal group: 90 mmol / kg
[0266] (PA-8) Polyamide 66
[0267] VN (sulfuric acid): 124 ml / g, amino terminal group: 46 mmol / kg, carboxylic acid terminal group: 78 mmol / kg
[0268] (Component (B) and component (D))
[0269] (B) Component: Cuprous iodide (manufactured by Wako Pure Chemical Industries, Ltd., hereinafter referred to as CuI)
[0270] (D) Component: Potassium iodide (manufactured by Wako Pure Chemical Industries, Ltd., hereinafter referred to as KI)
[0271] A mixture of component (B): component (D) = 1:5 (mass ratio)
[0272] ((C) ingredient: glass fiber)
[0273] (GF-1) Product name: ECS10-03-568H (manufactured by Jushi Group Co., Ltd.)
[0274] Boron element: 0.0 mass%, Mg / Si ratio: 0.02, Fe element: 0.34 mass%, Na element: 1.03 mass%
[0275] (GF-2) Product name: ECS301HP-3-H (Chongqing International Composite Materials Co., Ltd.)
[0276] Boron element: 0.0 mass%, Mg / Si ratio: 0.07, Fe element: 0.50 mass%, Na element: 1.5 mass%
[0277] (GF-3) Trade name: HP-3610 (manufactured by Nippon Electric Glass Co., Ltd.)
[0278] Boron element: 0.0 mass%, Mg / Si ratio: 0.17, Fe element: 0.56 mass%, Na element: 0.56 mass%
[0279] (GF-4) Trade name: ECS03T-275H (manufactured by Nippon Electric Glass Co., Ltd.)
[0280] Boron element: 2.0 mass%, Mg / Si ratio: 0.03, Fe element: 0.17 mass%, Na element: 1.8 mass%
[0281] (GF-5) Trade name: CS983-10P (Owens Corning Corporation)
[0282] Boron element: 0.0%, Mg / Si ratio: 0.00, Fe element: 0.30 mass%, Na element: 1.34 mass%
[0283] ((E) ingredient: colorant)
[0284] (E-1) Trade name: Pigment Orange 43 (manufactured by Clariant Chemicals, pigment colorant)
[0285] (E-2) Trade name: CI Solvent Orange 60 (manufactured by LANXESS, dye-based colorant)
[0286] [Examples 1 to 17 and 20 to 25] [Comparative Examples 1 to 12]
[0287] A twin-screw extruder [ZSK-26MC, manufactured by Coperion (Germany)] having an upstream supply port in the first barrel from the upstream side of the extruder and a downstream supply port in the ninth barrel with L / D (barrel length of the extruder / barrel diameter of the extruder) = 48 (number of barrels: 12) was used.
[0288] In the twin-screw extruder, the following settings were made: the temperature from the upstream supply port to the die was 290° C., the screw rotation speed was 250 rpm, and the discharge amount was 25 kg / hour.
[0289] Under these conditions, (A-1) main component polyamide (PA-1, PA-2, PA-3, PA-4, PA-5, PA-6), (B) a mixture of component (D), and (A-2) different types of polyamide (PA-3, PA-4, PA-5, PA-6) were supplied from the upstream supply port in the proportions shown in Tables 1 to 8 below, and (C) component (GF-1, GF-2, GF-3, GF-4, GF-5) was supplied from the downstream supply port.
[0290] Then, these materials were melt-kneaded to produce pellets of polyamide resin compositions of Examples 1 to 17 and 20 to 25 and Comparative Examples 1 to 12. In the following table, "normal" in the kneading strength means that the processing resin temperature during extrusion rotation is less than 355°C, and "strong kneading" means that the processing resin temperature during extrusion rotation is 355°C or more.
[0291] Using the obtained polyamide resin composition (pellet), the weight average fiber length of the component (C) was determined by the above-mentioned method.
[0292] [Table 1]
[0293]
[0294] [Table 2]
[0295]
[0296] [Table 3]
[0297]
[0298] [Table 4]
[0299]
[0300] [Table 5]
[0301]
[0302] [Table 6]
[0303]
[0304] [Table 7]
[0305]
[0306] [Table 8]
[0307]
[0308] The obtained pellets were used to evaluate tensile strength, tensile strength after heat aging, tensile strength after heat aging per 1 part by mass of glass fiber, flexural strength, Charpy impact strength, and color tone change by the above-mentioned methods.
[0309] The evaluation results are shown in Tables 9 to 16 below.
[0310] The larger the tensile strength before heat aging, the better the mechanical strength (mechanical properties).
[0311] The greater the tensile strength and retention rate after heat aging, the more excellent the heat aging resistance is.
[0312] The greater the bending strength, the more excellent the rigidity is.
[0313] A larger Charpy impact strength indicates better toughness (mechanical properties).
[0314] The smaller the color difference ΔE* in the color tone change, the smaller the change in color tone corresponding to the change in water content, indicating that the visibility is excellent.
[0315] [Table 9]
[0316]
[0317] [Table 10]
[0318]
[0319] [Table 11]
[0320]
[0321] [Table 12]
[0322]
[0323] [Table 13]
[0324]
[0325] [Table 14]
[0326]
[0327] [Table 15]
[0328]
[0329] [Table 16]
[0330]
[0331] The evaluation results are as follows: For the test pieces made from the polyamide resin compositions of Examples 1 to 17 and 20 to 25, discoloration due to moisture was suppressed while maintaining mechanical properties and heat aging resistance, compared with the test pieces made from the polyamide resin compositions of Comparative Examples 1 to 12.
[0332] [Examples 18 and 19]
[0333] Pellets of the polyamide resin compositions of Examples 18 and 19 were produced in the same manner as in Example 1, except that the (A-1) main component polyamide (PA-1), the mixture of the (B) component and the (D) component, and the (E) colorant were supplied from the upstream supply port, and the (C) component was supplied from the downstream supply port, respectively, in accordance with the ratios described in Table 17 below.
[0334] [Table 17]
[0335]
[0336] The obtained pellets were used to evaluate tensile strength, flexural strength, Charpy impact strength and discoloration change by the above method. Examples 18 and 19 have the same composition as Example 3 except that the processing resin temperature is slightly different and a colorant is used, so it is believed that the same behavior and tendency as Example 3 are shown in terms of heat aging resistance.
[0337] The evaluation results are shown in Table 18 below.
[0338] [Table 18]
[0339]
[0340] The evaluation results showed that the change in color tone of Example 18 using a pigment-based colorant was smaller (ΔE* was smaller) than that of Example 19 using a dye-based colorant, and that discoloration was suppressed.
[0341] Industrial Applicability
[0342] According to the present invention, a polyamide resin composition can be provided which can suppress discoloration (fading) due to moisture while maintaining mechanical properties and high heat aging resistance. In addition, a molded body can be provided which uses such a polyamide resin composition as a material and can suppress discoloration due to moisture while maintaining mechanical properties and high heat aging resistance.
Claims
1. A polyamide resin composition, It is characterized in that The polyamide resin composition comprises: 100 parts by mass of (A) polyamide resin, 0.005 to 0.3 parts by mass of (B) a copper compound, 10 to 250 parts by mass of (C) glass fibers, The content of the boron element in the glass fiber (C) is 1% by mass or less relative to the total mass of the glass fiber (C).
2. The polyamide resin composition according to claim 1, in, The (A) polyamide resin is one or more selected from the group consisting of polyamides and copolyamides, The polyamide is selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I and polyamide MXD6, The copolyamide is a copolymer including at least one selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 4T, polyamide 6T, polyamide 6I, and polyamide MXD6 as a constituent component.
3. The polyamide resin composition according to claim 2, in, The (A) polyamide resin comprises (A-1) a main component polyamide and at least one (A-2) different type of polyamide.
4. The polyamide resin composition according to claim 3, in, The molecular weight of the (A-2) different type of polyamide is smaller than the molecular weight of the (A-1) main component polyamide.
5. The polyamide resin composition according to claim 3, in, The content of the (A-2) different type of polyamide is 0.01 to 10 parts by mass in 100 parts by mass of the (A) polyamide resin.
6. The polyamide resin composition according to claim 1, It is characterized in that The polyamide resin composition further contains (D) at least one of an alkali metal halide and an alkaline earth metal halide, The molar ratio of the content of the (D) halogen compound to the content of the (B) copper compound is 2 / 1 to 50 / 1.
7. The polyamide resin composition according to claim 1, in, The ratio (Mg / Si) of the magnesium (Mg) element to the silicon (Si) element in the (C) glass fiber is 0.01 to 0.
2.
8. The polyamide resin composition according to claim 1, in, The content of iron in the glass fiber (C) is 0.01% by mass to 2.0% by mass relative to the total mass of the glass fiber (C).
9. The polyamide resin composition according to claim 1, in, The content of the sodium element in the glass fiber (C) is 0.1% by mass to 3.0% by mass relative to the total mass of the glass fiber (C).
10. The polyamide resin composition according to claim 1, in, The polyamide resin composition further contains 0.01 to 5 parts by mass of (E) a colorant based on 100 parts by mass of the polyamide resin composition.
11. The polyamide resin composition according to claim 10, in, The (E) colorant includes at least one selected from the group consisting of titanium oxide, zinc sulfide, zinc oxide, iron oxide, and organic dyes.
12. The polyamide resin composition according to claim 11, It is characterized in that The (E) colorant includes at least one orange colorant.
13. A shaped body, in, The molded body comprises the polyamide resin composition according to any one of claims 1 to 10.
14. A shaped body, in, The molded body comprises the polyamide resin composition according to claim 11.
15. A shaped body, in, The molded body comprises the polyamide resin composition according to claim 12.
16. The molded article according to claim 13, in, The molded body is an automobile part.
17. The molded article according to claim 14 or 15, in, The molded body is an automobile part.
18. A polyamide resin composition, comprising: 100 parts by mass of (A) polyamide resin, 0.005 to 0.3 parts by mass of (B) a copper compound, 10 to 60 parts by weight of (C) glass fibers, in, The polyamide resin composition has a tensile strength after heat aging of 3.0 or more, measured by the following method, per 1 part by mass of the glass fiber. (Tensile strength after heat aging) A multi-purpose test piece (type A) produced by a method according to ISO 3167 using the polyamide resin composition was heat aged in a hot air circulation oven at 200° C. for 1,000 hours. The test piece after heat aging was cooled at 23° C. for 24 hours or more, and then subjected to a tensile test at a tensile speed of 5 mm / min by a method according to ISO527, and the tensile strength (MPa) after heat aging was measured.