Modified attapulgite-based starch microspheres as well as preparation method and application thereof
By combining modified attapulgite with silane quaternary ammonium salts, starch microspheres with high adsorption capacity and drug loading capacity are prepared, which solves the problems of insufficient adsorption capacity and drug loading capacity of existing starch microspheres and realizes the realization of microspheres. Good dispersion and drug payload.
Patent Information
- Application Number
- CN202410964522.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
Existing starch microspheres have insufficient adsorption capacity and drug loading capacity, are prone to agglomeration, and have poor dispersion, making it difficult to meet the needs of efficient drug carriers and adsorbents.
Modified attapulgite is combined with silane quaternary ammonium salt, and the modified attapulgite is prepared by purifying and acidifying the attapulgite and silane quaternary ammonium salt. Starch and cross-linking agent are added, and modified attapulgite-based starch microspheres are prepared by spray drying. , forming microspheres with excellent adsorption capacity and drug loading capacity.
The adsorption capacity, drug loading capacity and dispersion capacity of starch microspheres are significantly improved. The drug loading capacity can reach 164.8mg/g, the adsorption capacity reaches 157.6mg/g, and the agglomeration rate is only 1.3%, ensuring drug payload and sustained release.
Smart Images

Figure CN118725356A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to modified attapulgite-based starch microsphere and a preparation method thereof, belonging to the technical field of starch microsphere. Background Art
[0002] Starch is a naturally renewable, low-cost and sustainable polysaccharide, and is considered to be an alternative material for industrial polymers. In recent years, it has been found that starch-based microspheres prepared with starch as raw material have many advantages and uses. For example, starch microspheres have been used as drug carriers for targeted preparations in the fields of nasal drug delivery systems, arterial embolization technology, radiotherapy, and immunoassays due to their biocompatibility, biodegradability, non-toxicity, storage stability, wide sources of raw materials, and low prices. Starch microspheres can also be used as adsorbents and embedding agents to adsorb or embed other substances besides drugs, such as flavors, fragrances, enzymes, and spores; cross-linked starch microspheres also have broad application prospects in the fields of metal ion adsorption and separation or wastewater treatment.
[0003] At present, starch microspheres can be prepared by physical method, chemical method and reverse microemulsion method. The reverse microemulsion method is a new method for preparing nano starch microspheres, which can be divided into two categories: one is to first disperse the aqueous phase of the starch solution in the oil phase to make an oil-in-water reverse microemulsion, and then add an appropriate amount of crosslinking agent to crosslink the polymer chains of the starch into spheres; the other method is to introduce unsaturated bonds on the starch molecules to form sites for free radical attack, and then use an initiator to initiate free radical polymerization to generate microspheres, but this method takes a long time. At present, the most commonly used method is the first method to prepare starch microspheres. The process is to dissolve starch in water, disperse it as an aqueous phase in an organic solution containing an appropriate amount of surfactant to form a uniform, stable and transparent microemulsion. Under rapid stirring, add an appropriate amount of crosslinking agent to crosslink the dissolved starch molecules into fine microspheres that precipitate from the liquid phase. On the basis of starch microspheres, adding other matrices can further improve the performance of starch microspheres.
[0004] Among them, attapulgite clay is widely used in environmental protection, food, medicine, etc. due to its many properties such as adsorption performance, rheological properties and carrier properties. Therefore, attapulgite can be added to starch microspheres to improve the drug loading and adsorption performance of starch microspheres. However, the adsorption capacity and drug loading of attapulgite in the prior art still need to be improved, and the prepared starch microspheres are easy to agglomerate and have poor dispersibility.
[0005] Therefore, there is an urgent need for a kind of attapulgite-based starch microspheres with excellent adsorption capacity, drug loading capacity and strong dispersion ability. Summary of the invention
[0006] Purpose of the invention: The first purpose of the present invention is to provide a modified attapulgite-based starch microsphere, the second purpose of the present invention is to provide a method for preparing the modified attapulgite-based starch microsphere, and the third purpose of the present invention is to provide the use of the modified attapulgite-based starch microsphere as a drug carrier in pharmaceutical manufacturing.
[0007] Technical solution: The invention comprises modified attapulgite, starch and a cross-linking agent; the modified attapulgite is prepared by reacting the purified and acidified attapulgite with a silane quaternary ammonium salt;
[0008] The structure of the silane quaternary ammonium salt is shown in the following formula A:
[0009]
[0010] Furthermore, the modified attapulgite-based starch microspheres contain, by mass percentage, 15-20% of modified attapulgite, 3-5% of a cross-linking agent, and the remainder being starch.
[0011] Furthermore, the cross-linking agent is selected from one of epichlorohydrin, phosphorus oxychloride or glutaraldehyde.
[0012] Furthermore, the silane quaternary ammonium salt is prepared by using 4-bromo-N,N-bis(trimethylsilyl)aniline, dodecyldimethyl tertiary amine and allyl 2-ethyl bromoacetate as raw materials.
[0013] Furthermore, the preparation method of the silane quaternary ammonium salt comprises the following steps:
[0014] (1) 4-bromo-N,N-bis(trimethylsilyl)aniline, sodium hydroxide and an organic solvent are stirred and mixed uniformly, heated under nitrogen protection, dodecyldimethyl tertiary amine is added, the temperature is kept for reaction, the organic solvent is removed, and recrystallization is performed to obtain a silane intermediate;
[0015] (2) The silane intermediate and the organic solvent are stirred and mixed uniformly, the temperature is raised under nitrogen protection, allyl 2-bromoacetic acid ethyl ester is added, the temperature is kept for reaction, the organic solvent is removed, the mixture is cooled, filtered, washed, and dried to obtain the silane quaternary ammonium salt.
[0016] Furthermore, in step (1), the molar ratio of 4-bromo-N,N-bis(trimethylsilyl)aniline to dodecyldimethyl tertiary amine is 1:1.2-1.5.
[0017] Furthermore, in step (1), the temperature is raised to 70-80° C. under nitrogen protection, and the reaction time is kept at this temperature for 18-24 hours.
[0018] Furthermore, in step (2), in the silicon step (2), the molar ratio of the silane intermediate to allyl 2-bromoacetate is 1:1.1-1.3.
[0019] Furthermore, in step (2), the temperature is raised to 60-70° C. under nitrogen protection, and the insulation reaction time is 6-12 hours.
[0020] Furthermore, in step (1) and step (2), the organic solvent is N,N-dimethylformamide, tetrahydrofuran, dichloromethane or N,N-dimethylacetamide.
[0021] The method for preparing the modified attapulgite-based starch microspheres of the present invention comprises the following steps:
[0022] (1) adding attapulgite to deionized water, stirring, standing and settling, removing lower layer impurities and supernatant, filtering by suction, and drying to obtain purified attapulgite;
[0023] (2) adding purified attapulgite and dilute sulfuric acid to deionized water, stirring, filtering, washing until the filtrate is neutral, and drying to obtain acidified attapulgite;
[0024] (3) adding the acidified attapulgite and silane quaternary ammonium salt into deionized water, performing ultrasonic dispersion, heating and stirring to react, cooling, filtering, washing, and drying to obtain modified attapulgite;
[0025] (4) Add starch and a cross-linking agent into deionized water, stir and mix to gelatinize, add modified attapulgite, stir and mix evenly, and spray dry to obtain modified attapulgite-based starch microspheres.
[0026] Furthermore, in step (1) and step (2), the stirring is carried out at 100 to 200 r / min for 16 to 24 hours.
[0027] Furthermore, in step (1), the static sedimentation time is 16 to 24 hours.
[0028] Furthermore, in step (2), the concentration of dilute sulfuric acid is 30-65%.
[0029] Furthermore, in step (2), the mass ratio of purified attapulgite, dilute sulfuric acid and deionized water is (10-15): (5-8): (40-50).
[0030] Furthermore, in step (3), the mass ratio of acidified attapulgite, silane quaternary ammonium salt and deionized water is (10-15): (8-10): (40-50).
[0031] Furthermore, in step (3), the ultrasonic dispersion time is 1 to 2 hours.
[0032] Furthermore, in step (3), the temperature of the heating and stirring reaction is 60 to 70° C., and the time of the heating and stirring reaction is 1 to 2 hours.
[0033] The present invention also includes the use of the modified attapulgite-based starch microspheres as drug carriers in pharmaceutical manufacturing.
[0034] The silane quaternary ammonium salt of the present invention has excellent dispersibility and pore-forming ability. On the one hand, the silane quaternary ammonium salt has a long-chain alkyl structure with hydrophobic ability and a plurality of quaternary ammonium structures with hydrophilic ability, so that the silane quaternary ammonium salt has excellent surface activity, and can effectively disperse the prepared starch microspheres in various media, avoid agglomeration between the starch microspheres, and effectively improve the dispersibility of the starch microspheres. On the other hand, the multi-branched silane structure can form a network structure by cross-linking in a small area during the formation of the starch microspheres, and further form a large number of stable and uniform pore structures in the starch microspheres, thereby improving the specific surface area of the starch microspheres, thereby further improving the adsorption capacity and drug loading of the starch microspheres.
[0035] The silane quaternary ammonium salt with unsaturated bonds in the present invention can be effectively grafted onto the surface of the acidified attapulgite to modify it. The modified attapulgite can further improve the adsorption capacity, drug loading capacity and dispersion capacity of the starch microspheres, and its quaternary ammonium salt structure can give the starch microspheres a certain bactericidal ability, thereby improving the safety of the starch microspheres.
[0036] In the present invention, by adding attapulgite material with good adsorption and carrier capacity into starch microspheres, the adsorption capacity of starch microspheres can be effectively improved, and the starch microspheres can be endowed with the ability to carry drugs through adsorption, thereby avoiding the problem of drug failure during the preparation process of starch microspheres.
[0037] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0038] (1) The starch microspheres prepared by modifying attapulgite with silane quaternary ammonium salt having unsaturated bonds can have a drug loading of up to 164.8 mg / g, an adsorption capacity of up to 157.6 mg / g, and an agglomeration rate of only 1.3%. The adsorption capacity, drug loading and dispersion capacity of the starch microspheres are greatly improved, and the starch microspheres can effectively complete the tasks of adsorption, drug loading and sustained release, and can be widely used in the field of starch microsphere technology.
[0039] (2) The preparation method of the present invention can form a large number of stable and uniform pore structures in the prepared starch microspheres, have a large specific surface area, and have a stable structure. A large amount of drugs can be loaded and maintained stable, which can avoid the problem of drug failure during the preparation process of starch microspheres.
[0040] (3) The modified attapulgite-based starch microspheres provided by the present invention use attapulgite modified with silane quaternary ammonium salt as a matrix and add an appropriate amount of cross-linking agent, which can not only make the prepared starch microspheres have a large number of pore structures, expand the specific surface area of the starch microspheres, and increase the drug loading amount, but also the attapulgite structure modified with silane quaternary ammonium salt can further improve the adsorption capacity of the starch microspheres and the dispersion capacity between the starch microspheres, so that the starch microspheres can effectively complete the tasks of adsorption, drug loading and sustained release, and can be widely used in the field of starch microsphere technology. DETAILED DESCRIPTION
[0041] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0042] Among them, the commercially available starch microspheres are porous magnetic composite microspheres purchased from Xi'an Qiyue Biotechnology Co., Ltd.; the remaining reagents and equipment are conventional reagents and equipment in this technical field.
[0043] Example 1
[0044] 1. Preparation of silane quaternary ammonium salt
[0045] (1) In a reactor, 0.03 mol of 4-bromo-N,N-bis(trimethylsilyl)aniline, 0.5 g of sodium hydroxide and 50 mL of N,N-dimethylformamide were added, stirred and mixed evenly, heated to 75° C. under nitrogen protection, 0.04 mol of dodecyldimethyl tertiary amine was added, and the reaction was kept warm for 24 hours, and N,N-dimethylformamide was removed by reduced pressure distillation at 70-90° C., and a silane intermediate was obtained after recrystallization;
[0046] The product silane intermediate was analyzed by LC-MS, and the mass spectrum data of the product were m / z 449.37 (100.0%), 450.38 (39.6%), 451.38 (14.1%), 452.38 (3.2%);
[0047] (2) Add 0.02 mol of silane intermediate and 100 mL of N,N-dimethylformamide to the reactor, stir and mix evenly, heat to 65° C. under nitrogen protection, add 0.025 mol of allyl 2-bromoacetate, keep the temperature for reaction for 8 hours, remove N,N-dimethylformamide by vacuum distillation at 70-90° C., cool, filter, wash and dry to obtain silane quaternary ammonium salt;
[0048] The product silane quaternary ammonium salt was analyzed by LC-MS, and the mass data of the product were m / z 548.42 (100.0%), 549.42 (45.5%), 550.42 (16.7%), and 551.42 (4.1%).
[0049] From the above data, it can be seen that the structure of silane quaternary ammonium salt is shown in the following formula A:
[0050]
[0051] 2. Preparation of modified attapulgite-1
[0052] (1) Add 30 g of attapulgite and 200 mL of deionized water into a reactor, stir at 150 r / min for 24 h, let it stand for 24 h, remove the impurities in the lower layer and the supernatant, repeat the above steps 3 times, filter and dry to obtain purified attapulgite;
[0053] (2) In a reactor, 15 g of purified attapulgite, 5 g of 60% by mass dilute sulfuric acid and 50 mL of deionized water were added, and the mixture was stirred at 200 r / min for 24 h, then filtered, washed with deionized water until the filtrate was neutral, and dried to obtain acidified attapulgite;
[0054] (3) In a reactor, 15 g of acidified attapulgite, 10 g of the silane quaternary ammonium salt obtained in step 1 and 50 mL of deionized water were added, and the mixture was ultrasonically dispersed for 2 h and then heated to 70° C., stirred for reaction for 2 h, cooled, filtered, washed with deionized water, and dried to obtain the modified attapulgite-1.
[0055] 3. Preparation of modified attapulgite-based starch microspheres
[0056] In a reactor, 78 parts of starch, 4 parts of epichlorohydrin and 200 parts of deionized water are added in a weight ratio, stirred and mixed, and then gelatinized, and 18 parts of modified attapulgite-1 are added, stirred and mixed evenly, and then spray-dried to obtain the modified attapulgite-based starch microspheres; that is, the modified attapulgite-based starch microspheres contain, based on a total mass fraction of 100%, 18% of modified attapulgite-1, 4% of epichlorohydrin, and the remainder is starch.
[0057] Example 2
[0058] The experimental process is basically the same as Example 1, except that in step 3, epichlorohydrin is replaced by phosphorus oxychloride, and 80 parts of starch, 5 parts of phosphorus oxychloride, 200 parts of deionized water, and 15 parts of modified attapulgite-1 are added in a weight ratio to prepare modified attapulgite-based starch microspheres, that is, the modified attapulgite-based starch microspheres contain, based on a total mass fraction of 100%, 15% of modified attapulgite-1, 5% of phosphorus oxychloride, and the remainder is starch.
[0059] Example 3
[0060] The experimental process is basically the same as Example 1, except that in step 3, epichlorohydrin is replaced by glutaraldehyde, and 77 parts of starch, 3 parts of phosphorus oxychloride, 200 parts of deionized water, and 20 parts of modified attapulgite-1 are added by weight to prepare modified attapulgite-based starch microspheres, that is, the modified attapulgite-based starch microspheres contain, based on a total mass fraction of 100%, 20% of modified attapulgite-1, 3% of glutaraldehyde, and the remainder is starch.
[0061] Comparative Example 1
[0062] Commercially available starch microspheres were used directly.
[0063] Comparative Example 2
[0064] The experimental process of starch microspheres is basically the same as step 3 in Example 1, except that the modified attapulgite-1 is replaced with an equal amount of starch to obtain starch microspheres.
[0065] Comparative Example 3
[0066] The starch microsphere experimental process is basically the same as step 3 in Example 1, except that the modified attapulgite-1 is replaced by an equal amount of attapulgite. The obtained attapulgite-based starch microspheres contain 18% of modified attapulgite-2, 4% of epichlorohydrin, and the remainder of starch, based on a total mass fraction of 100%.
[0067] Comparative Example 4
[0068] (1) Preparation of modified concave clay-2
[0069] The modified attapulgite experimental process is basically the same as the preparation of modified attapulgite-1 in step 2 of Example 1, except that the silane quaternary ammonium salt in step (3) of step 2 is replaced by an equal amount of sodium dodecylbenzene sulfonate. Step 3 is the same as step 3 of Example 1, and modified attapulgite-1 is replaced by an equal amount of modified attapulgite-2. The modified attapulgite-based starch microspheres obtained contain 18% of modified attapulgite-2, 4% of epichlorohydrin, and the remainder is starch, based on a total mass fraction of 100%.
[0070] Example 4 Performance Test
[0071] Drug loading capacity test: 10 mg of the products of Examples 1-3 and Comparative Examples 1-4 were dispersed into 1 mL of a 2 mg / mL doxorubicin hydrochloride solution, and after standing for 20 minutes, the concentration of doxorubicin hydrochloride remaining in the solution was detected using a spectrophotometer at a wavelength of 470 nm. The drug loading of the product was calculated according to drug loading = drug mass in starch microspheres / starch microsphere mass -1. The results are shown in Table 1.
[0072] Adsorption capacity test: 10 mg of the products of Examples 1-3 and Comparative Examples 1-4 were dispersed into 1 mL of 2 mg / mL doxorubicin hydrochloride solution, left to stand for 20 minutes and then shaken at 100 rpm for 24 hours, and then the concentration of doxorubicin hydrochloride remaining in the solution was detected by a spectrophotometer at a wavelength of 470 nm. The drug loading of the product was calculated according to drug loading = drug mass in starch microspheres / starch microsphere mass - 2. The results are shown in Table 1.
[0073] Dispersibility test: 1 g of the products of Examples 1-3 and Comparative Examples 1-4 were placed in 50 mL of deionized water, shaken at 100 rpm for 30 minutes, filtered, and the agglomerated products were weighed and the agglomeration rate was calculated. Agglomeration rate (%) = precipitate weight / total product mass * 100%, the results are shown in Table 1.
[0074] Table 1 Performance data of starch microspheres
[0075] Drug loading-1(mg / g) Drug loading-2(mg / g) Agglomeration rate (%) Example 1 164.3 157.4 1.3 Example 2 162.7 155.6 1.2 Example 3 164.8 157.6 1.3 Comparative Example 1 89.4 69.6 8.4 Comparative Example 2 81.2 64.3 9.2 Comparative Example 3 134.8 117.5 5.7 Comparative Example 4 138.7 125.1 4.1
[0076] As can be seen from Table 1, according to the comparison of the test results of Examples 1-3 with those of Comparative Example 1, the modified attapulgite-based starch microspheres provided by the present invention have better drug loading capacity and adsorption capacity than the starch microspheres in the prior art, and have strong dispersion ability, which can avoid the agglomeration of starch microspheres.
[0077] According to the comparison of the test results of Examples 1-3 and Comparative Example 2, adding modified attapulgite to the modified attapulgite-based starch microspheres provided by the present invention can significantly improve the drug loading capacity, adsorption capacity and dispersion capacity of the starch microspheres.
[0078] According to the comparison of the test results of Examples 1-3 and Comparative Examples 3-4, it can be seen that in the modified attapulgite-based starch microspheres provided by the present invention, by adding attapulgite modified with silane quaternary ammonium salt, the drug loading capacity, adsorption capacity and dispersion capacity of the starch microspheres can be further improved, and the silane quaternary ammonium salt has better dispersion ability and pore-forming ability than the surfactant in the prior art.
[0079] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A modified attapulgite-based starch microsphere, characterized in that: The invention comprises modified attapulgite, starch and a cross-linking agent; the modified attapulgite is prepared by reacting the purified and acidified attapulgite with a silane quaternary ammonium salt; The structure of the silane quaternary ammonium salt is shown in the following formula A:
2. The modified attapulgite-based starch microspheres according to claim 1, characterized in that: The modified attapulgite-based starch microspheres contain, by mass percentage, 15-20% of modified attapulgite, 3-5% of a cross-linking agent, and the remainder being starch.
3. The modified attapulgite-based starch microspheres according to claim 1, characterized in that: The cross-linking agent is selected from one of epichlorohydrin, phosphorus oxychloride or glutaraldehyde.
4. The modified attapulgite-based starch microspheres according to claim 1, characterized in that: The silane quaternary ammonium salt is prepared by using 4-bromo-N, N-bis(trimethylsilyl)aniline, dodecyldimethyl tertiary amine and allyl 2-ethyl bromoacetate as raw materials.
5. The modified attapulgite-based starch microspheres according to claim 4, characterized in that: The preparation method of the silane quaternary ammonium salt comprises the following steps: (1) 4-bromo-N,N-bis(trimethylsilyl)aniline, sodium hydroxide and an organic solvent are stirred and mixed uniformly, heated under nitrogen protection, dodecyldimethyl tertiary amine is added, the temperature is kept for reaction, the organic solvent is removed, and recrystallization is performed to obtain a silane intermediate; (2) The silane intermediate and the organic solvent are stirred and mixed uniformly, the temperature is raised under nitrogen protection, allyl 2-bromoacetic acid ethyl ester is added, the temperature is kept for reaction, the organic solvent is removed, the mixture is cooled, filtered, washed, and dried to obtain the silane quaternary ammonium salt.
6. The modified attapulgite-based starch microspheres according to claim 5, characterized in that: In step (1), the molar ratio of 4-bromo-N,N-bis(trimethylsilyl)aniline to dodecyldimethyl tertiary amine is 1:1.2-1.5, the temperature is raised to 70-80°C under nitrogen protection, and the heat preservation reaction time is 18-24 hours.
7. The modified attapulgite-based starch microspheres according to claim 5, characterized in that: In step (2), the molar ratio of the silane intermediate to allyl 2-bromoacetic acid ethyl ester is 1:1.1-1.3, the temperature is raised to 60-70°C under nitrogen protection, and the insulation reaction time is 6-12 hours. In step (1) and step (2), the organic solvent is N,N-dimethylformamide, tetrahydrofuran, dichloromethane or N,N-dimethylacetamide.
8. The method for preparing modified attapulgite-based starch microspheres according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) adding attapulgite to deionized water, stirring, standing and settling, removing lower layer impurities and supernatant, filtering by suction, and drying to obtain purified attapulgite; (2) adding purified attapulgite and dilute sulfuric acid to deionized water, stirring, filtering, washing until the filtrate is neutral, and drying to obtain acidified attapulgite; (3) adding the acidified attapulgite and silane quaternary ammonium salt into deionized water, performing ultrasonic dispersion, heating and stirring to react, cooling, filtering, washing, and drying to obtain modified attapulgite; (4) Add starch and a cross-linking agent into deionized water, stir and mix to gelatinize, add modified attapulgite, stir and mix evenly, and spray dry to obtain modified attapulgite-based starch microspheres.
9. The method for preparing modified attapulgite-based starch microspheres according to claim 8, characterized in that: In step (1) and step (2), stirring is carried out at 100-200 r / min for 16-24 hours; in step (1), the static sedimentation time is 16-24 hours; in step (2), the concentration of dilute sulfuric acid is 30-65%, the mass ratio of purified attapulgite, dilute sulfuric acid and deionized water is (10-15): (5-8): (40-50); in step (3), the mass ratio of acidified attapulgite, silane quaternary ammonium salt and deionized water is (10-15): (8-10): (40-50), the ultrasonic dispersion time is 1-2 hours, the temperature of the heated stirring reaction is 60-70°C, and the heated stirring reaction time is 1-2 hours.
10. Use of the modified attapulgite-based starch microspheres according to any one of claims 1 to 7 as a drug carrier in pharmaceutical manufacturing.
Citation Information
Cited By
Silicon-free water-soluble core mold material and preparation method thereof
CN121446962A