Preparation process of composite material of graphite and hard carbon coated nano silicon
Through the composite material preparation process of graphite and hard carbon-coated nano-silicon, the problems of agglomeration and volume expansion of nano-silicon particles are solved, the dispersion and cycle life of the battery are improved, and more stable battery performance is achieved.
Patent Information
- Application Number
- CN202410989811.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When nano-silicon is used as anode material for lithium-ion batteries, its high surface energy causes particle agglomeration, making it difficult to control dispersion, and volume expansion causes SEI film growth, affecting battery life.
The composite material preparation process of graphite and hard carbon coating nano-silicon is used to form a multi-layer coating structure through ultrasonic dispersion, dry coating and high-temperature carbonization, which reduces the surface energy and volume expansion of nano-silicon and improves dispersion and structural stability. .
It significantly improves the dispersion uniformity of nano-silicon and battery cycle life, extends the slurry storage period, and enhances the battery's charge and discharge capacity and structural stability.
Smart Images

Figure CN118738346A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary battery material preparation, and more specifically, relates to a preparation process of a composite material of graphite and hard carbon-coated nano-silicon. Background Art
[0002] When nano silicon particles are used as negative electrode materials for lithium-ion batteries, they have a higher theoretical capacity than common graphite negative electrode materials. Their room temperature theoretical capacity can be as high as 3580mAh / g, which is almost ten times that of graphite. However, when a single silicon material is directly used as a negative electrode material, there are many problems. For example, due to its low conductivity, this may lead to poor electron transmission efficiency during the battery charging and discharging process; and the volume expansion of silicon during the charging and discharging process is high, up to 300%, which may cause its particles to pulverize and fall off, thereby reducing the product cycle life; furthermore, the SEI film formed by silicon particles during the initial formation process of the battery will continue to grow due to the expansion of the volume, resulting in the continuous consumption of electrolyte and active lithium, affecting the battery cycle life.
[0003] Although nano-sizing of silicon particles can solve the above problems to a certain extent, for example, it can alleviate the volume expansion of silicon particles; however, after nano-sizing, the surface energy of silicon particles is relatively high, and the particles are easy to agglomerate, especially when they are dispersed into negative electrode active slurry and coated, the dispersion uniformity of the particles is difficult to control, resulting in uncontrolled uniformity of the electrode. Summary of the invention
[0004] The technical problem to be solved by the present invention is: when nano-silicon is used as a negative electrode material, the surface energy of silicon particles is high and the particles are easy to agglomerate, which makes it difficult to control the consistency of product processing. In addition, during the actual use of the product, the repeated expansion of the silicon particles will lead to the continuous growth of the SEI film, which ultimately affects the service life of the product. A preparation process for a composite material of graphite and hard carbon coated nano-silicon is provided.
[0005] The purpose of the present invention is to provide a preparation process of a composite material of graphite and hard carbon coated nano-silicon.
[0006] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0007] A preparation process of a composite material of graphite and hard carbon coated nano-silicon, the specific preparation process comprising:
[0008] Dispersion of Nano-Silicon:
[0009] After mixing the nano silicon powder, the first dispersant and the first dispersing medium, the nano silicon powder is evenly dispersed by ultrasonic to obtain a nano silicon dispersion;
[0010] Dispersion of natural graphite:
[0011] After mixing natural graphite, a second dispersant and a second dispersion medium, the mixture is uniformly dispersed by ultrasonication to obtain a natural graphite dispersion;
[0012] Raw material blending:
[0013] The nano-silicon dispersion and the natural graphite dispersion are uniformly mixed, dried, and crushed to obtain a mixed powder;
[0014] Dry coating of raw materials:
[0015] After mixing the mixed powder and the coating material, stirring and coating to obtain the coating material;
[0016] Carbonization:
[0017] The coating material is carbonized at high temperature under the protection of inert gas, cooled and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
[0018] Furthermore, the first dispersant is selected from any one of hexadecyltrimethylammonium chloride, polyvinyl alcohol, and sodium lignin sulfonate; the second dispersant is selected from any one of hexadecyltrimethylammonium chloride, polyvinyl alcohol, and sodium lignin sulfonate; the first dispersion medium is selected from any one of ethanol, methanol, n-hexane, n-propanol, and isopropanol; the second dispersion medium is selected from any one of ethanol, methanol, n-hexane, n-propanol, and isopropanol.
[0019] Furthermore, the coating material is selected from any one of coal tar or petroleum tar.
[0020] Furthermore, the nano silicon powder is silicon powder with a D50 of 50-200nm.
[0021] Furthermore, the natural graphite is natural flake graphite with a D50 of 8-30 μm.
[0022] Furthermore, the dispersion of the nano-silicon further comprises:
[0023] After mixing nano silicon powder, single-walled carbon nanotubes, a first dispersant and a first dispersion medium, the mixture is evenly dispersed by ultrasonication to obtain a nano silicon dispersion;
[0024] The average length of the single-walled carbon nanotubes is 5-20 μm; and the amount of the single-walled carbon nanotubes is 3-5% of the mass of the nano-silicon powder.
[0025] Furthermore, the specific preparation process includes:
[0026] Dispersion of Nano-Silicon:
[0027] By weight, 10-15 parts of nano silicon powder, 1-2 parts of the first dispersant and 100-120 parts of the first dispersion medium are mixed, and then ultrasonically dispersed to obtain a nano silicon dispersion;
[0028] Dispersion of natural graphite:
[0029] By weight, 15-20 parts of natural graphite, 1-2 parts of a second dispersant and 100-120 parts of a second dispersion medium are mixed, and then ultrasonically dispersed to obtain a natural graphite dispersion;
[0030] Raw material blending:
[0031] The nano-silicon dispersion and the natural graphite dispersion are mixed uniformly in a mass ratio of 1:(2.2-2.5), dried, and crushed to obtain a mixed powder;
[0032] Dry coating of raw materials:
[0033] The mixed powder and the coating material are mixed in a mass ratio of 10:(0.6-0.8), and then stirred and coated to obtain the coating material.
[0034] Beneficial effects:
[0035] (1) The present invention uses natural graphite and hard carbon to coat the nano-silicon material layer by layer, thereby forming a multi-layer coating structure with nano-silicon as the core, natural graphite as the middle coating layer, and the surface coating layer as hard carbon, and the hard carbon coating layer is obtained by high-temperature carbonization. In addition, during the dry coating process, part of the natural graphite is bonded to each other with the help of a hard carbon precursor (asphalt). In this way, during the carbonization process, part of the natural graphite is connected and fixed by hard carbon. Therefore, the surface cavities or nanopores formed by the hard carbon material during the carbonization process can be relied on to smoothly realize the infiltration of the electrolyte from the surface of the material to the inside, so that the material as a whole shows good compatibility with the electrolyte, thereby ensuring the performance of the material during use; in addition, during the battery charging and discharging process, the hard carbon can serve as a skeleton to effectively support the stability of the overall structure and avoid the structural collapse problem caused by excessive expansion of nano-silicon;
[0036] Furthermore, thanks to the coating of natural graphite and hard carbon, the surface energy of nano silicon particles can be significantly reduced, so that the product can be stably dispersed in the solvent during processing, avoiding the gelation of the negative electrode slurry, extending the turnover period of the slurry during storage, and also improving the dispersion uniformity of the slurry on the surface of the negative electrode current collector during the coating process to a certain extent;
[0037] (2) Further, by adjusting the usage ratio of natural graphite, nano-silicon, and coating material (asphalt) during the preparation process, the ratio of natural graphite coating layer, hard carbon coating layer and inner core nano-silicon in the final composite material can be adjusted. This is because the inventors found that within this ratio range, a relatively thin hard carbon coating layer can be formed on the graphite surface. The reason for controlling the coating amount of the surface hard carbon is that the hard carbon has more functional groups on the surface during the carbonization process. Although the presence of these functional groups is helpful for the compatibility between the material and the electrolyte, if there are too many functional groups, it is easy to cause the material to inevitably undergo adsorption and sedimentation during the preparation of the negative electrode slurry, thereby causing the storage stability of the slurry to decrease, or the viscosity is too high, resulting in difficulty in controlling the coating uniformity on the collector surface; but if there are too few functional groups, it is easy to cause the material to have limited force as a skeleton material, and the material structure is easy to collapse during rapid charge and discharge;
[0038] (3) In addition, the inventors further discovered that in the process of mixed coating of nano-silicon and natural graphite, since the nano-silicon particles are small and spherical or quasi-spherical, the contact points between them and the flaky natural graphite are small, while the single-walled carbon nanotubes have excellent flexibility. When the single-walled carbon nanotubes with a length greater than that of silicon micropowder are selected, they can be effectively connected or filled between the nano-silicon particles and the natural graphite coating layer, which can serve as a link for structural stability and significantly reduce the product DCR, thereby reducing the polarization here and improving the battery charging and discharging capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a SEM image of the composite material of graphite and hard carbon-coated nano-silicon prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0041] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0042] Example 1
[0043] Dispersion of Nano-Silicon:
[0044] After mixing 10 parts of nano silicon powder, 1 part of the first dispersant and 100 parts of the first dispersion medium by weight, adding single-walled carbon nanotubes of 3% by weight of the nano silicon powder, and performing ultrasonic dispersion for 180 minutes at a temperature of 35° C. and an ultrasonic frequency of 70 kHz to obtain a nano silicon dispersion;
[0045] The nano silicon powder is selected from silicon micropowder with a D50 of 50nm;
[0046] The average length of the single-walled carbon nanotubes is 5 μm;
[0047] Dispersion of natural graphite:
[0048] After mixing 15 parts of natural graphite, 1 part of the second dispersant and 100 parts of the second dispersion medium by weight, the mixture was ultrasonically dispersed for 180 minutes at a temperature of 35° C. and an ultrasonic frequency of 90 kHz to obtain a natural graphite dispersion;
[0049] The natural graphite is natural flake graphite with a D50 of 8 μm;
[0050] The first dispersant is selected from hexadecyl trimethyl ammonium chloride; the second dispersant is selected from hexadecyl trimethyl ammonium chloride; the first dispersing medium is selected from ethanol; the second dispersing medium is selected from ethanol;
[0051] Raw material blending:
[0052] The nano-silicon dispersion and the natural graphite dispersion were mixed at a mass ratio of 1:2.2, and the mixture was continuously stirred at 800 r / min for 2 h with a stirrer, and then filtered to collect the filter cake, and then the obtained filter cake was transferred to an oven and dried to constant weight at 100°C, and then the dried filter cake was transferred to a universal grinder and crushed, and then passed through a 400-mesh sieve to obtain a mixed powder;
[0053] Dry coating of raw materials:
[0054] The mixed powder and coating material were mixed in a mass ratio of 10:0.6 and poured into a coating machine. They were first stirred at a low speed of 300 r / min for 30 minutes, and then stirred at a high speed of 1500 r / min for dry coating to obtain the coating material.
[0055] The coating material is selected from coal tar;
[0056] Carbonization:
[0057] The coated material is transferred into a carbonization furnace, and an inert gas is introduced into the furnace to replace the air. Then, the temperature is raised to 1200°C at a rate of 1°C / min under the protection of the inert gas. After carbonization for 4 hours, the material is cooled to room temperature with the furnace and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
[0058] The inert gas is selected from nitrogen.
[0059] Example 2
[0060] Dispersion of Nano-Silicon:
[0061] By weight, 12 parts of nano silicon powder, 1.5 parts of the first dispersant and 110 parts of the first dispersion medium were mixed, and then single-walled carbon nanotubes (4% by weight of the nano silicon powder) were added, and ultrasonic dispersion was performed for 190 minutes at a temperature of 35° C. and an ultrasonic frequency of 75 kHz to obtain a nano silicon dispersion;
[0062] The nano silicon powder is selected from silicon micropowder with a D50 of 80nm;
[0063] The average length of the single-walled carbon nanotubes is 10 μm;
[0064] Dispersion of natural graphite:
[0065] After mixing 18 parts of natural graphite, 1.5 parts of the second dispersant and 110 parts of the second dispersion medium by weight, the mixture was ultrasonically dispersed for 190 minutes at a temperature of 35° C. and an ultrasonic frequency of 95 kHz to obtain a natural graphite dispersion;
[0066] The natural graphite is natural flake graphite with a D50 of 18 μm;
[0067] The first dispersant is selected from polyvinyl alcohol; the second dispersant is selected from hexadecyltrimethylammonium chloride; the first dispersing medium is selected from n-hexane; the second dispersing medium is selected from n-propanol;
[0068] Raw material blending:
[0069] The nano-silicon dispersion and the natural graphite dispersion were mixed at a mass ratio of 1:2.4, and the mixture was continuously stirred and mixed at a speed of 1000 r / min for 2.5 h, and then filtered to collect the filter cake. The filter cake was then transferred to an oven and dried to constant weight at a temperature of 100°C. The dried filter cake was then transferred to a universal grinder and crushed, and then passed through a 600-mesh sieve to obtain a mixed powder.
[0070] Dry coating of raw materials:
[0071] The mixed powder and coating material were mixed in a mass ratio of 10:0.7 and poured into a coating machine. They were first stirred at a low speed of 300 r / min for 30 minutes, and then stirred at a high speed of 1500 r / min for dry coating to obtain the coating material.
[0072] The coating material is selected from petroleum asphalt;
[0073] Carbonization:
[0074] The coated material is transferred into a carbonization furnace, and an inert gas is introduced into the furnace to replace the air. Then, the temperature is raised to 1300°C at a rate of 3°C / min under the protection of the inert gas. After carbonization for 6 hours, the material is cooled to room temperature with the furnace and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
[0075] The inert gas is selected from argon.
[0076] Example 3
[0077] Dispersion of Nano-Silicon:
[0078] After mixing 15 parts of nano silicon powder, 2 parts of the first dispersant and 120 parts of the first dispersion medium by weight, adding single-walled carbon nanotubes of 5% by weight of the nano silicon powder, and performing ultrasonic dispersion for 200 minutes at a temperature of 35° C. and an ultrasonic frequency of 80 kHz to obtain a nano silicon dispersion;
[0079] The nano silicon powder is selected from silicon micropowder with a D50 of 200 nm;
[0080] The average length of the single-walled carbon nanotubes is 20 μm;
[0081] Dispersion of natural graphite:
[0082] After mixing 20 parts of natural graphite, 2 parts of the second dispersant and 120 parts of the second dispersion medium by weight, the mixture was ultrasonically dispersed for 200 minutes at a temperature of 35° C. and an ultrasonic frequency of 100 kHz to obtain a natural graphite dispersion;
[0083] The natural graphite is natural flake graphite with a D50 of 30 μm;
[0084] The first dispersant is selected from sodium hexadecyl lignin sulfonate; the second dispersant is selected from polyvinyl alcohol; the first dispersing medium is selected from ethanol; the second dispersing medium is selected from methanol;
[0085] Raw material blending:
[0086] The nano-silicon dispersion and the natural graphite dispersion were mixed at a mass ratio of 1:2.5, and the mixture was continuously stirred at a speed of 1200 r / min for 3 hours, and then filtered to collect the filter cake. The filter cake was then transferred to an oven and dried to a constant weight at a temperature of 100°C. The dried filter cake was then transferred to a universal grinder and crushed, and then passed through an 800-mesh sieve to obtain a mixed powder.
[0087] Dry coating of raw materials:
[0088] The mixed powder and coating material were mixed in a mass ratio of 10:0.8 and poured into a coating machine. They were first stirred at a low speed of 300 r / min for 30 minutes, and then stirred at a high speed of 1500 r / min for dry coating to obtain the coating material.
[0089] The coating material is selected from coal tar;
[0090] Carbonization:
[0091] The coated material is transferred into a carbonization furnace, and an inert gas is introduced into the furnace to replace the air. Then, the temperature is raised to 1500°C at a rate of 5°C / min under the protection of the inert gas. After carbonization for 10 hours, the material is cooled to room temperature with the furnace and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
[0092] The inert gas is selected from nitrogen.
[0093] Example 4
[0094] The present embodiment differs from the embodiment 1 in that no single-walled carbon nanotubes are added, and the other conditions remain unchanged.
[0095] Example 5
[0096] The difference between this embodiment and embodiment 1 is that the average length of the single-walled carbon nanotubes is 45 nm, and the other conditions remain unchanged.
[0097] Example 6
[0098] Compared with Example 1, this embodiment is different in that:
[0099] Raw material blending:
[0100] The nano-silicon dispersion and the natural graphite dispersion were mixed at a mass ratio of 1:2, and the mixture was continuously stirred at a speed of 800 r / min for 2 h, and then filtered to collect the filter cake. The filter cake was then transferred to an oven and dried to a constant weight at a temperature of 100°C. The dried filter cake was then transferred to a universal grinder and crushed, and passed through a 400-mesh sieve to obtain a mixed powder.
[0101] Dry coating of raw materials:
[0102] The mixed powder and coating material were mixed in a mass ratio of 10:2 and poured into a coating machine. They were first stirred at a low speed of 300 r / min for 30 min, and then stirred at a high speed of 1500 r / min for dry coating to obtain the coating material.
[0103] The coating material is selected from coal tar.
[0104] Comparative Example 1
[0105] Compared with Example 1, this comparative example has the following differences:
[0106] Carbonization:
[0107] The coated material is transferred into a carbonization furnace, and an inert gas is introduced into the furnace to replace the air. Then, the temperature is raised to 700°C at a rate of 1°C / min under the protection of the inert gas. After carbonization for 4 hours, the material is cooled to room temperature with the furnace and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
[0108] The inert gas is selected from nitrogen.
[0109] Since the carbonization temperature is significantly lower than that of Example 1, no hard carbon is formed during the carbonization process of this comparative example.
[0110] Comparative Example 2
[0111] The difference between this comparative example and Example 1 is that no natural graphite is added, and the other conditions remain unchanged.
[0112] Silicon powder with a D50 of 50 nm was used as the negative electrode active material without any treatment.
[0113] The performance tests were performed on the products obtained in Examples 1-6 and Comparative Examples 1-2. The specific test methods and test results are as follows:
[0114] Slurry storage stability test:
[0115] The products obtained in the above different embodiments or comparative examples were respectively prepared into negative electrode slurries. Specifically, the formula was: composite material: binder sodium carboxymethyl cellulose: thickener SBR: solvent water = 90:3:2:120. After being stirred and mixed evenly with a stirrer at a speed of 800 r / min, the slurries were left to stand at room temperature. After 72 hours, the stored slurries were observed to see if obvious sedimentation occurred. The detailed results are shown in Table 1:
[0116] Table 1: Product storage stability test results
[0117] Is there any significant subsidence? Example 1 no Example 2 no Example 3 no Example 4 no Example 5 no Example 6 no Comparative Example 1 no Comparative Example 2 yes Blank example yes
[0118] Cycle performance test:
[0119] The products obtained in the above embodiments or comparative examples were used as negative electrode active materials, respectively. The negative electrode active material, conductive carbon black Super-P and carboxymethyl cellulose were mixed in a mass ratio of 9:0.5:0.5, and deionized water was added as a solvent. The mixture was stirred at a speed of 300 r / min for 12 hours to prepare a negative electrode slurry. Subsequently, the negative electrode slurry was scraped on the surface of the copper foil, and dried at 100° C. for 12 hours to obtain a negative electrode sheet, which was then cut after rolling. The compaction density of the active material on the surface of the negative electrode sheet was controlled at 1.65 g / cm 3 ;
[0120] With lithium nickel cobalt manganese oxide (NCM811) as the positive electrode active material, the positive electrode active material, the conductive agent acetylene black and PVDF are mixed in a mass ratio of 95:3:2, and NMP is used as the solvent to prepare the positive electrode slurry, which is then coated on the surface of aluminum foil and dried, and then rolled and cut to obtain the positive electrode sheet. The compaction density of the active material on the surface of the positive electrode sheet is controlled at 3.8g / cm 3 ;
[0121] Use polyethylene film as the diaphragm;
[0122] In an argon atmosphere glove box, organic solvents ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) were mixed evenly in a volume ratio of 1 / 1 / 1, 1 mol / L LiPF6 lithium salt was added and dispersed evenly, and then 5% fluoroethylene carbonate was dissolved in the above organic solvents, and stirred evenly to obtain an electrolyte;
[0123] The prepared positive electrode sheet, negative electrode sheet and separator are made into corresponding electrode assemblies according to the Z-shaped stacking structure. The electrode assembly is vacuum dried at 90℃ for 12h, and then the positive and negative electrode tabs are ultrasonically welded. The positive electrode uses aluminum tabs and the negative electrode uses nickel tabs. The positive and negative electrode tabs are located on the same side of the electrode assembly. The electrode assembly after the tabs are welded is placed in an aluminum-plastic film of appropriate size for top and side sealing. The top and side sealing temperature is 145℃, and then the electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery then undergoes static, hot and cold pressing, formation, shaping, capacity testing and other processes in sequence to obtain a battery cell.
[0124] The obtained single battery was charged at 0.5C current at 25°C until the charging voltage reached 4.25V, and then continued to charge at a constant voltage until the current reached 0.05C, at which time the charging was stopped, and it was considered fully charged; then the single battery was discharged at 1C current until the voltage reached 2.7V, at which time the discharging was stopped, and it was considered fully discharged;
[0125] The battery is fully charged and discharged until it decays to less than 80% of its initial capacity, which is considered the end of its life and the cycle life is 1.
[0126] Another batch of batteries were prepared according to the above battery preparation process. The obtained single batteries were charged at 2C current at 25°C until the charging voltage reached 4.25V, and then continued to charge at a constant voltage until the current reached 0.05C, at which time the charging was stopped, and it was considered fully charged; then the single batteries were discharged at 1C current until the voltage reached 2.7V, at which time the discharging was stopped, and it was considered fully discharged;
[0127] The battery is fully charged and discharged until it decays to less than 80% of its initial capacity, which is considered the end of its life, and the cycle life is 2.
[0128] The specific test results are shown in Table 2:
[0129] Table 2: Product cycle performance test results
[0130] Cycle life 1 / circle Cycle life 2 / circle Example 1 2255 1650 Example 2 2262 1667 Example 3 2271 1672 Example 4 2090 1380 Example 5 2167 1425 Example 6 2135 1421 Comparative Example 1 1980 1191 Comparative Example 2 1678 890 Blank example 1520 850
[0131] It can be seen from the test results in Table 2 that the product obtained by the present invention has excellent cycle performance, and can still obtain relatively excellent cycle performance under large current charge and discharge conditions.
[0132] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A process for preparing a composite material of graphite and hard carbon coated nano-silicon, characterized in that: The specific preparation process includes: Dispersion of Nano-Silicon: After mixing the nano silicon powder, the first dispersant and the first dispersing medium, the nano silicon powder is evenly dispersed by ultrasonic to obtain a nano silicon dispersion; Dispersion of natural graphite: After mixing natural graphite, a second dispersant and a second dispersion medium, the mixture is uniformly dispersed by ultrasonication to obtain a natural graphite dispersion; Raw material blending: The nano-silicon dispersion and the natural graphite dispersion are uniformly mixed, dried, and crushed to obtain a mixed powder; Dry coating of raw materials: After mixing the mixed powder and the coating material, stirring and coating to obtain the coating material; Carbonization: The coating material is carbonized at high temperature under the protection of inert gas, cooled and discharged to obtain a composite material of graphite and hard carbon coated nano-silicon.
2. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 1, characterized in that: The first dispersant is selected from any one of hexadecyltrimethylammonium chloride, polyvinyl alcohol, and sodium lignin sulfonate; the second dispersant is selected from any one of hexadecyltrimethylammonium chloride, polyvinyl alcohol, and sodium lignin sulfonate; the first dispersing medium is selected from any one of ethanol, methanol, n-hexane, n-propanol, and isopropanol; the second dispersing medium is selected from any one of ethanol, methanol, n-hexane, n-propanol, and isopropanol.
3. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 1, characterized in that: The coating material is selected from any one of coal tar or petroleum tar.
4. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 1, characterized in that: The nano silicon powder is silicon powder with a D50 of 50-200 nm.
5. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 1, characterized in that: The natural graphite is natural flake graphite with a D50 of 8-30 μm.
6. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 4, characterized in that: The dispersion of the nano-silicon further comprises: After mixing nano silicon powder, single-walled carbon nanotubes, a first dispersant and a first dispersion medium, the mixture is evenly dispersed by ultrasonication to obtain a nano silicon dispersion; The average length of the single-walled carbon nanotubes is 5-20 μm; and the amount of the single-walled carbon nanotubes is 3-5% of the mass of the nano-silicon powder.
7. The process for preparing a composite material of graphite and hard carbon coated nano-silicon according to claim 1, characterized in that: The specific preparation process comprises: Dispersion of Nano-Silicon: By weight, 10-15 parts of nano silicon powder, 1-2 parts of the first dispersant and 100-120 parts of the first dispersion medium are mixed, and then ultrasonically dispersed to obtain a nano silicon dispersion; Dispersion of natural graphite: By weight, 15-20 parts of natural graphite, 1-2 parts of a second dispersant and 100-120 parts of a second dispersion medium are mixed, and then ultrasonically dispersed to obtain a natural graphite dispersion; Raw material blending: The nano-silicon dispersion and the natural graphite dispersion are mixed uniformly in a mass ratio of 1:(2.2-2.5), dried, and crushed to obtain a mixed powder; Dry coating of raw materials: The mixed powder and the coating material are mixed in a mass ratio of 10:(0.6-0.8), and then stirred and coated to obtain the coating material.
Citation Information
Patent Citations
Preparation method of silicon carbon composite material
CN109473664A
Silicon-carbon composite lithium ion battery negative electrode material and preparation method thereof
CN110707314A
Nanometer silicon composite negative electrode active material, preparation method, pole piece and lithium ion battery
CN115692638A
Nanometer silicon / biomass hard carbon / graphite composite negative electrode material and preparation method and application thereof
CN117059785A
Silicon-carbon negative electrode material and preparation method thereof
CN117497735A
Cited By
Preparation process and application of nano silicon-carbon composite graphite material
CN121192150A