Lithium iron phosphate / lithium vanadium phosphate superstructure solid solution as well as autocatalytic preparation method and application thereof

Through lithium iron phosphate/lithium vanadium phosphate superstructure solid solution and autocatalytic preparation methods, nano-vanadium trioxide is used to improve the electrochemical performance of lithium battery materials, solve the problem of insufficient performance of traditional lithium iron phosphate materials, and achieve high-efficiency Lithium battery power materials.

CN118738384AActive Publication Date: 2024-10-01SHANDONG XIEHE UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410882777.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

The electrochemical performance of traditional lithium iron phosphate materials has not yet reached a satisfactory level, especially in terms of charge and discharge rates, power density and cycle stability. There is room for improvement.

Method used

Using lithium iron phosphate/lithium vanadium phosphate superstructure solid solution x LiFePO4·(1-x)Li3V2(PO4)3, and through the autocatalytic preparation method, using nano-vanadium trioxide as the autocatalytic guide, and obtained by sintering and sieving Highly efficient lithium iron phosphate/lithium vanadium phosphate superstructure solid solution.

Benefits of technology

Significantly improve the charge and discharge rate, power density and cycle stability, improve the electrochemical properties of the material, and achieve higher energy efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738384A_ABST
    Figure CN118738384A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium battery power materials, in particular to a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution and a preparation method and application thereof. The lithium iron phosphate / lithium vanadium phosphate superstructure solid solution provided by the invention is xLiFePO4. (1-x) Li3V2 (PO4) 3, wherein x is more than 0.5 and less than 0.95; the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution provided by the invention has the advantages of relatively high charge-discharge rate, high power density, good cycle stability and relatively high energy efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery power materials, and in particular to a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution and an autocatalytic preparation method and application thereof. Background Art

[0002] Lithium-ion batteries have become the mainstream of power tools due to their high energy, high power, environmental protection and multiple recycling characteristics.

[0003] Lithium iron phosphate material is currently the main lithium battery power material, with the advantages of good safety, long service life and low cost. However, the electrochemical performance of traditional lithium iron phosphate materials needs to be improved. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution and its autocatalytic preparation method and application. The lithium iron phosphate / lithium vanadium phosphate superstructure solid solution provided by the present invention has the advantages of high charge and discharge rate, high power density, good cycle stability and high energy efficiency.

[0005] In order to achieve the above objectives, the present invention provides the following technical solutions.

[0006] The present invention provides a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution, wherein the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is x LiFePO4·(1-x)Li3V2(PO4)3; wherein 0.5<x<0.95.

[0007] Preferably, the particle size of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is less than 200 mesh.

[0008] The present invention discloses a method for preparing a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution by autocatalysis, comprising the following steps:

[0009] Mixing lithium carbonate, iron phosphate, a vanadium source and an autocatalytic guide to obtain a mixture; the vanadium source includes nano vanadium trioxide; the autocatalytic guide is one or more of vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone;

[0010] sintering the mixed material to obtain a preliminary material;

[0011] The preliminary material is sieved, and the material under the sieve is taken to obtain the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution.

[0012] Preferably, the sintering temperature is 700-900° C., and the holding time is 9-11 hours.

[0013] Preferably, the sieve particle size is 200 mesh.

[0014] Preferably, the molar ratio of the iron in the iron phosphate to the vanadium in the vanadium source is (0.5-0.95):(1-0.1); the molar ratio of the lithium in the lithium carbonate to the iron in the iron phosphate is 1:1.

[0015] Preferably, the mass of the autocatalytic guide agent is 0.5-3% of the total mass of the lithium carbonate, iron phosphate and vanadium source.

[0016] Preferably, the mixing method is stirring; and the mixing time is 2 to 3 hours.

[0017] The present invention also provides the use of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution described above or the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution prepared by the preparation method described in the above technical scheme in lithium battery power materials.

[0018] The present invention provides a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution, wherein the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is x LiFePO4·(1-x)Li3V2(PO4)3; wherein 0.5<x<0.95. The lithium iron phosphate / lithium vanadium phosphate superstructure solid solution of the present invention contains lithium vanadium phosphate (Li3V2(PO4)3); the introduction of lithium vanadium phosphate (Li3V2(PO4)3) can increase the charge and discharge rate, increase the power density, improve the cycle stability, increase the energy efficiency, and improve the electrochemical performance of the material.

[0019] The present invention also provides a method for preparing the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution described above, comprising the following steps: mixing lithium carbonate, iron phosphate, a vanadium source and an autocatalytic guide to obtain a mixture; the vanadium source includes nano vanadium trioxide; the autocatalytic guide is one or more of vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone; sintering the mixture to obtain a preliminary material; sieving the preliminary material, taking the sieve under the sieve to obtain the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution. In the present invention, first, the nano vanadium trioxide (reactant and autocatalyst) is guided as a crystal nucleus by the autocatalytic guide (vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone) to promote the rapid crystallization of lithium iron phosphate and shorten the synthesis cycle. Second, the nano vanadium trioxide can also be used as a raw material and a catalyst at the same time, as a new crystal nucleus to catalyze itself to react with lithium iron phosphate to generate a fast ion lithium vanadium phosphate (Li3V2(PO4)3). The introduction of fast ions (Li3V2(PO4)3) can increase the charge and discharge rate, increase the power density, improve the cycle stability, increase the energy efficiency, and improve the electrochemical performance of the material. Third, nano-vanadium trioxide will also promote the reaction of lithium iron phosphate and lithium vanadium phosphate, speed up the material synthesis time, and finally prepare the target product x LiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Example 1;

[0021] Figure 2 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Example 2:

[0022] Figure 3 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Example 3. DETAILED DESCRIPTION

[0023] The present invention provides a lithium iron phosphate / lithium vanadium phosphate superstructure solid solution, wherein the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is x LiFePO4·(1-x)Li3V2(PO4)3; wherein 0.5<x<0.95.

[0024] In the present invention, the particle size of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is preferably less than 200 mesh.

[0025] The present invention also provides a method for preparing the above-mentioned lithium iron phosphate / lithium vanadium phosphate superstructure solid solution, comprising the following steps:

[0026] Mixing lithium carbonate, iron phosphate, a vanadium source and an autocatalytic guide to obtain a mixture; the vanadium source includes nano vanadium trioxide; the autocatalytic guide is one or more of vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone;

[0027] sintering the mixed material to obtain a preliminary material;

[0028] The preliminary material is sieved, and the material under the sieve is taken to obtain the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution.

[0029] The invention mixes lithium carbonate, iron phosphate and a vanadium source to obtain a mixed material.

[0030] In the present invention, the vanadium source includes nano vanadium trioxide; the autocatalytic guide is preferably one or more of vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone, more preferably vanadium acetylacetonate or vanadium acylhydrazone.

[0031] In the present invention, the molar ratio of the iron in the iron phosphate to the vanadium in the vanadium source is preferably (0.5-0.95): (1-0.1), more preferably 0.8:0.4; the molar ratio of the lithium in the lithium carbonate to the iron in the iron phosphate is preferably 1: 1. In the present invention, the mass of the autocatalytic guide is preferably 0.5-3% of the total mass of the lithium carbonate, the iron phosphate and the vanadium source, more preferably 1-2%.

[0032] In the present invention, the mixing method is preferably stirring, the stirring speed is preferably 200 to 600 rpm, more preferably 450 rpm, and the stirring time is preferably 2 to 3 hours, more preferably 2.5 hours.

[0033] After obtaining the mixed material, the present invention sintered the mixed material to obtain a preliminary material.

[0034] In the present invention, the sintering temperature is preferably 700-900°C, more preferably 750-850°C, and the holding time is preferably 9-11h, more preferably 10h. In the present invention, the heating rate to the sintering temperature is preferably 2-15°C / min, more preferably 8°C / min.

[0035] In the present invention, after the sintering, cooling is further included, and the cooling is preferably cooled to room temperature.

[0036] After obtaining the preliminary material, the present invention sieves the preliminary material, takes the sieve under material, and obtains the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution.

[0037] In the present invention, the particle size of the sieve is preferably 200 mesh.

[0038] The present invention also provides the use of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution described above or the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution prepared by the preparation method described in the above technical scheme in lithium battery power materials.

[0039] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0040] Example 1

[0041] Lithium carbonate and iron phosphate are used as raw materials, nano vanadium trioxide is used as raw material and catalyst, vanadium acetylacetonate is used as catalyst guide, and the molar ratio of iron in iron phosphate, lithium in lithium carbonate, and vanadium in nano vanadium trioxide is 0.8:0.8:0.4, and vanadium acetylacetonate is 1% of the total mass of lithium carbonate, iron phosphate and nano vanadium trioxide; the materials are mixed for 3 hours under stirring conditions of 450rpm. The mixed materials are placed in a roasting furnace for sintering at a temperature of 800℃ (heating rate of 8℃ / min) for 9h to obtain a preliminary product; the preliminary product is passed through a 200-mesh standard sieve, and the sieve-under material is taken to obtain a xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution, wherein x=0.8.

[0042] Figure 1 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 solid solution prepared in Example 1. Figure 1 It can be seen that the material was successfully prepared with regular shape and uniform particle size.

[0043] Example 2

[0044] Lithium carbonate and iron phosphate are used as raw materials, nano vanadium trioxide is used as raw material and catalyst, acetylacetonate vanadium is used as catalyst guide, and the molar ratio of iron in iron phosphate, lithium in lithium carbonate, and vanadium in nano vanadium trioxide is 0.7:0.7:0.4, and acetylacetonate vanadium is 2% of the total mass of lithium carbonate, iron phosphate and nano vanadium trioxide. The materials are mixed for 3 hours under stirring conditions of 450rpm. The mixed materials are placed in a roasting furnace for sintering at a temperature of 800℃ (heating rate of 8℃ / min) for 9 hours to obtain a preliminary product; the preliminary product is passed through a 200-mesh standard sieve, and the sieve-under material is taken to obtain a xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution, wherein x=0.7.

[0045] Figure 2 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Example 2. Figure 2 It can be seen that the material was successfully prepared, with a relatively regular shape and uniform particle size, but with a small amount of agglomeration.

[0046] Example 3

[0047] Lithium carbonate, iron phosphate and nano-vanadium trioxide are used as raw materials, acylhydrazone vanadium is used as a catalyst guide, and the molar ratio of iron in iron phosphate, lithium in lithium carbonate and vanadium in nano-vanadium trioxide is 0.6:0.6:0.4, and acylhydrazone vanadium is 2% of the total mass of lithium carbonate, iron phosphate and nano-vanadium trioxide. The mixture is mixed for 2 hours under stirring conditions of 400rpm. The mixture is placed in a roasting furnace for sintering at a temperature of 750℃ (heating rate of 8℃ / min) for 9 hours to obtain a preliminary product; the preliminary product is passed through a 200-mesh standard sieve, and the sieve-under material is taken to obtain a xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution, wherein x=0.6.

[0048] Figure 3 This is the SEM image of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Example 3. Figure 3 It can be seen that the material was successfully prepared, but the shape and particle size were quite different.

[0049] The present invention also tests the electrochemical properties (charge and discharge rate, power density, cycle stability, energy efficiency) of the xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solution prepared in Examples 1 to 3. The test method is as follows: the electrochemical performance test is performed using a 2032 button cell. The mass ratio of the prepared active material xLiFePO4·(1-x)Li3V2(PO4)3, the conductive agent (acetylene black) and the binder (PVDF) is 8:1:1, the electrolyte is 1 mol / L LiPF6, EC+DEC (volume ratio 1:1), and the test environment temperature is constant at 25°C. The test results are shown in Table 1.

[0050] Table 1 Electrochemical properties of xLiFePO4·(1-x)Li3V2(PO4)3 superstructure solid solutions of Examples 1 to 3

[0051]

[0052] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A lithium iron phosphate / lithium vanadium phosphate solid solution, It is characterized in that The lithium iron phosphate / lithium vanadium phosphate superstructure solid solution is xLiFePO 4 ·(1-x)Li 3 V 2 (PO 4 ) 3 ; where 0.5<x<0.

95.

2. The lithium iron phosphate / lithium vanadium phosphate superstructure solid solution according to claim 1, It is characterized in that The particle size of the lithium iron phosphate / lithium vanadium phosphate solid solution is less than 200 meshes.

3. The autocatalytic preparation method of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution according to claim 1, It is characterized in that The following steps are involved: Mixing lithium carbonate, iron phosphate, a vanadium source and an autocatalytic guide to obtain a mixture; the vanadium source includes nano vanadium trioxide; the autocatalytic guide is one or more of vanadium acetylacetonate, vanadium oxyacetylacetonate and vanadium acylhydrazone; The mixed material is sintered to obtain a preliminary material; The preliminary material is sieved, and the material under the sieve is taken to obtain the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution.

4. The autocatalytic preparation method according to claim 2, It is characterized in that The sintering temperature is 700-900° C., and the heat preservation time is 9-11 hours.

5. The autocatalytic preparation method according to claim 2, It is characterized in that The particle size of the sieve is 200 meshes.

6. The autocatalytic preparation method as claimed in claim 2, It is characterized in that The molar ratio of the iron in the iron phosphate to the vanadium in the vanadium source is (0.5-0.95):(1-0.1); the molar ratio of the lithium in the lithium carbonate to the iron in the iron phosphate is 1:

1.

7. The autocatalytic preparation method as claimed in claim 2, It is characterized in that The mixing method is stirring; the mixing time is 2 to 3 hours.

8. The autocatalytic preparation method as claimed in claim 2, It is characterized in that The mass of the self-catalytic guide agent is 0.5-3% of the total mass of the lithium carbonate, the iron phosphate and the vanadium source.

9. Use of the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution according to any one of claims 1 to 2 or the lithium iron phosphate / lithium vanadium phosphate superstructure solid solution prepared by the preparation method according to any one of claims 3 to 7 in lithium battery power materials.

Citation Information

Patent Citations

  • An anode material for compound lithium ion battery

    CN101262058A

  • Method for improving tap density of composite anode material xLiFePO4.yLi3V2(PO4)3 of lithium ion battery

    CN102244244A

  • Phosphate-coated nano-grade lithium iron phosphate cathode material and preparation method thereof

    CN102842713A

  • Lithium iron phosphate-lithium vanadium phosphate composite positive electrode material and preparation method and application thereof

    CN114300661A

  • Vanadium-based phosphate positive electrode material containing Mn and Al, preparation method of vanadium-based phosphate positive electrode material, battery and energy storage equipment

    CN116845230A