MOF-derived tungsten-doped ferronickel phosphide difunctional electrocatalyst and preparation method thereof
By growing NiFeMOF on the surface of nickel foam and performing tungsten-doped phosphating treatment, a tungsten-doped nickel iron phosphide electrocatalyst with good conductivity and many active sites was prepared, which solved the problem of insufficient conductivity and active sites of existing electrocatalysts. The scarcity problem improves the efficiency and industrial applicability of hydrogen production through electrolysis of water.
Patent Information
- Application Number
- CN202410829121.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-08
AI Technical Summary
When existing transition metal phosphides are used as bifunctional electrocatalysts, they have insufficient conductivity, small electrochemical specific surface area, and few exposed active sites, which affects the industrial-scale development of hydrogen production by electrolysis of water.
The MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst was prepared by in-situ growth of NiFeMOF nanosheet arrays on the surface of nickel foam, solvothermal treatment in sodium tungstate solution, and low-temperature phosphating method, and the surface chemistry of the catalyst was controlled. and electronic structure, increasing active sites and conductivity.
The catalytic activity and efficiency are significantly improved, the overpotential is reduced, and an electrocatalyst with good conductivity, high electrochemical specific surface area, and many exposed active sites is obtained, which is suitable for glucose electrocatalytic conversion coupled hydrogen production reaction and promotes industrial scale Development of hydrogen production by electrolysis of water.
Smart Images

Figure CN118745580A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic decomposition, and specifically relates to a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst and a preparation method thereof. Background Art
[0002] Hydrogen production by water electrolysis is considered to be an ideal hydrogen production technology, which mainly includes the oxygen evolution reaction (OER) at the anode and the hydrogen evolution reaction (HER) at the cathode. These two half reactions require a very high voltage to cross the reaction barrier, which consumes a lot of electricity. Precious metal catalysts are often used to reduce the overpotential required for the reaction. Furthermore, compared with precious metals, transition metals are more abundant and inexpensive, and their adjustable electronic structure can realize the construction of highly active and highly stable electrocatalysts, which can effectively reduce the energy required for the reaction.
[0003] The electrocatalytic oxygen evolution reaction occurs at the interface between the catalyst and the electrolyte, so the catalytic activity of the catalyst depends on its surface chemistry and electronic structure. Precisely controlling the surface chemical structure and electronic structure of the catalyst can significantly improve its intrinsic catalytic activity. In addition, increasing the contact area between the catalyst surface and the electrolyte can increase the effective utilization rate of the catalyst's active sites and the carrier density, thereby improving the catalytic activity.
[0004] At present, there have been a lot of reports on advanced transition metal-based catalysts replacing traditional precious metal catalysts for efficient water electrolysis systems, such as transition metal oxides, hydroxides, phosphides, sulfides, etc. Among them, transition metal phosphides (TMPs) can be used as bifunctional electrocatalysts for glucose electrocatalytic conversion coupled hydrogen production systems due to their good conductivity, mechanical strength and chemical stability. However, when current transition metal phosphides are used as bifunctional electrocatalysts, they have insufficient conductivity, small electrochemical specific surface area, and few exposed active sites, which affects the development of hydrogen production by water electrolysis on an industrial scale. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst and a preparation method, which has good catalytic activity and low price, can be used for the glucose electrocatalytic conversion coupled hydrogen production system, and has the advantages of good conductivity, high electrochemical specific surface area, and many exposed active sites.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst comprises the following steps:
[0008] S1, in situ growth of NiFeMOF nanosheet arrays on the surface of nickel foam to obtain NiFeMOF / NF;
[0009] S2, dissolving sodium tungstate in an ethanol solution to obtain a mixed solution, then immersing NiFeMOF / NF in the mixed solution for solvent thermal treatment, and then washing and drying to obtain tungsten-doped nickel-iron hydroxide;
[0010] S3, tungsten-doped nickel-iron hydroxide and sodium hypophosphite are heat-treated at 300-400° C. in a nitrogen atmosphere at a ratio of 0.05 mmol: (0.5-1.5) g to obtain a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst.
[0011] Preferably, S1 obtains NiFeMOF / NF according to the following process:
[0012] Nickel nitrate, ferric chloride and terephthalic acid were dissolved in a mixed solvent consisting of dimethylacetamide, deionized water and anhydrous ethanol, and the molar ratio of nickel nitrate, ferric chloride and terephthalic acid was 9:1:24 to obtain a mixed system. Nickel foam was impregnated into the mixed system, and the ratio of the upper surface area of the nickel foam to the nickel nitrate was 2 cm 2 : 0.15 mmol, and then a solvothermal reaction was carried out, and the obtained complex was washed and dried in sequence to obtain NiFeMOF / NF.
[0013] Furthermore, in the mixed solvent, the volume ratio of dimethylacetamide, deionized water and anhydrous ethanol is 28:1:1.
[0014] Preferably, the solvent thermal reaction is carried out at 120-160° C. for 4-8 hours.
[0015] Preferably, the molar ratio of sodium tungstate in S2 to nickel nitrate in S1 is 1:9, and tungsten-doped nickel-iron hydroxide is obtained.
[0016] Preferably, the solvent thermal treatment in S2 is carried out at 120-180° C. for 4-8 hours.
[0017] Preferably, the volume ratio of anhydrous ethanol to deionized water in the ethanol solution described in S2 is (5-25):(25-5), and the ratio of sodium tungstate to ethanol solution is 0.05mmol:30mL.
[0018] Preferably, when S3 is heat-insulating the tungsten-doped nickel-iron hydroxide and sodium hypophosphite, the temperature is heated from room temperature to 300 to 400° C. at a heating rate of 1 to 5° C. / min.
[0019] Preferably, S3 heats tungsten-doped nickel-iron hydroxide and sodium hypophosphite at 300-400° C. for 1-3 hours to obtain a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst.
[0020] A MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst obtained by the preparation method of the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst described in any one of the above.
[0021] Compared with the prior art, the present invention has the following beneficial technical effects:
[0022] The invention discloses a method for preparing a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst. The method comprises the following steps: performing solvent thermal treatment in an ethanol solution containing sodium tungstate to exchange tungsten ions, regulating the surface morphology and electronic structure of a NiFeMOF nanosheet array grown in situ on the surface of nickel foam, obtaining a tungsten-doped nickel-iron hydroxide, and finally regulating a suitable doping amount to prepare a MOF-derived tungsten-doped nickel-iron phosphide bifunctional catalyst by a low-temperature phosphating method, so that the positions originally occupied by hydrogen and oxygen elements are replaced by phosphorus elements, forming a new atomic coordination and electronic structure, and enriching the active sites of the catalyst. The obtained bifunctional electrocatalyst has good catalytic activity, high catalytic efficiency and low overpotential, can be used for glucose electrocatalytic conversion coupled hydrogen production reaction, has the advantages of good conductivity, high electrochemical specific surface area and many exposed active sites, and is of great significance for promoting the development of hydrogen production by electrolysis of water on an industrial scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a SEM image of the nickel foam-loaded NiFeMOF electrocatalyst obtained in Example 3 of the present invention.
[0024] Figure 2 This is a SEM image of the tungsten-doped nickel iron phosphide electrocatalyst derived from nickel foam supported MOF obtained in Example 3 of the present invention.
[0025] Figure 3 This is the full XPS spectrum of the tungsten-doped nickel iron phosphide electrocatalyst derived from nickel foam supported MOF obtained in Example 3 of the present invention.
[0026] Figure 4 This is a hydrogen evolution polarization curve of the tungsten-doped nickel-iron phosphide electrocatalyst derived from nickel foam supported MOF obtained in Example 3 of the present invention.
[0027] Figure 5 This is a graph showing the oxygen evolution polarization curve of the tungsten-doped nickel-iron phosphide electrocatalyst derived from the nickel foam-supported MOF obtained in Example 3 of the present invention.
[0028] Figure 6 This is a performance diagram of polarization curves of water electrolysis and glucose electrocatalytic conversion assisted electrolysis of water using the tungsten-doped nickel-iron phosphide electrocatalyst derived from MOF supported by nickel foam obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0030] The present invention provides a method for preparing a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst, which specifically comprises the following steps:
[0031] Step 1, using nickel nitrate and ferric chloride as metal sources, dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc (dimethylacetamide), deionized water and anhydrous ethanol in a volume ratio of 28 mL: 1 mL: 1 mL according to a molar ratio of 0.45 mmol: 0.05 mmol: 1.2 mmol. Then add a cleaned 2*3 cm 2 Nickel foam (NF, 1.7 mm thick sheet) was impregnated as a substrate, and the mixed system was transferred to a reactor for solvent thermal reaction at 120-160°C for 4-8 hours. Terephthalic acid was used as an organic ligand for self-assembly, and NiFeMOF nanosheet arrays were in situ grown on the surface of nickel foam. The obtained sample was washed with anhydrous ethanol and deionized water in turn, and vacuum dried to obtain NiFeMOF / NF, denoted as A.
[0032] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of (5-25): (25-5). Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 120-180°C for 4-8h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF, and the final material is recorded as B.
[0033] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 0.5-1.5 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and under nitrogen protection, heating at 300-400°C at a heating rate of 1-5°C / min for 1-3 hours from room temperature (phosphating treatment) to obtain a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0034] Example 1
[0035] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 120°C for 8 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0036] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 5:25. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 120°C for 8h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0037] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 0.5 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping them at 300°C for 3 hours at a heating rate of 5°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0038] Example 2
[0039] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 140°C for 6 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0040] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed liquid of anhydrous ethanol and deionized water in a volume ratio of 15:15. Immerse the NiFeMOF / NF obtained in step 1 in the mixed liquid. The mixed solution is subjected to solvent thermal treatment at 140°C for 6h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0041] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 1 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping them at 400°C for 3 hours at a heating rate of 5°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0042] Example 3
[0043] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 140°C for 6 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0044] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 15:15. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 160°C for 6h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0045] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 0.6 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping the temperature at 350°C for 2 hours at a heating rate of 3°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0046] from Figure 1 As shown in the SEM image, it can be seen that the nickel foam supported NiFeMOF electrocatalyst exhibits a microscopic morphology of nanosheet arrays.
[0047] from Figure 2 The SEM image shown shows that the MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst maintains the original nanosheet array morphology, while the spacing between the nanosheets is smaller.
[0048] from Figure 3 The full XPS spectrum shown shows that the MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst contains the elements Ni, Fe, W and P.
[0049] from Figure 4 The hydrogen evolution polarization curves shown in the figure show that the MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst exhibits excellent hydrogen evolution activity at a current density of 100 mA cm -2 When the voltage is 0.181 V, it is better than NiFeMOF / NF and close to commercial Pt / C.
[0050] from Figure 5As shown in the oxygen evolution polarization curve, the MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst exhibits excellent oxygen evolution activity at a current density of 100 mA cm -2 The voltage is only 1.47 V, which is better than NiFeMOF / NF and commercial RuO2.
[0051] from Figure 6 The polarization curve of the MOF-derived tungsten-doped nickel iron phosphide bifunctional electrocatalyst shows that when the electrolyte is 1M KOH solution, the electrolytic cell reaches 100mA / cm 2 The overpotential at 1.79V is 1.79V, at which time oxygen and hydrogen evolution reactions occur. When 50mM glucose is added to the electrolyte, the KOH concentration is also 1M, and the electrolytic cell reaches 100mA / cm 2 The overpotential at the anode is 1.56 V. Glucose, as the substrate for anodic oxidation, undergoes oxidation reaction at the anode and becomes an organic acid at the anode, avoiding the danger of mixing oxygen and hydrogen. Therefore, the electrocatalytic conversion reaction of glucose can significantly reduce the potential required by the electrolyzer, thereby reducing the energy consumption of hydrogen production.
[0052] Example 4
[0053] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 160°C for 4 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0054] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 10:20. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 180°C for 8h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0055] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 0.5 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping them at 400°C for 3 hours at a heating rate of 2°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0056] Example 5
[0057] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 160°C for 6 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0058] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 20:10. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 120°C for 8h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0059] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 1 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping the temperature at 350°C for 1 hour at a heating rate of 3°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0060] Example 6
[0061] Step 1, according to the amount of 0.45mmol, 0.05mmol, and 1.0mmol, nickel nitrate, ferric chloride, and terephthalic acid were dissolved in a mixed solution of DMAc, water, and anhydrous ethanol with a volume ratio of 28mL, 1mL, and 1mL, respectively. Then, a cleaned piece of 2*3cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 120°C for 4 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0062] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 5:25. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 140°C for 4h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0063] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 1 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping them at 300°C for 3 hours at a heating rate of 1°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
[0064] Example 7
[0065] Step 1: Dissolve nickel nitrate, ferric chloride and terephthalic acid in a mixed solution of DMAc, water and anhydrous ethanol with a volume of 28 mL, 1 mL and 1 mL, respectively, according to the dosage of 0.45 mmol, 0.05 mmol and 1.0 mmol, respectively. Then add a cleaned piece of 2*3 cm 2 The nickel foam was impregnated therein, and the mixed system was transferred to a reactor for solvent thermal reaction at 160°C for 6 hours. The obtained sample was washed with anhydrous ethanol and deionized water in turn and vacuum dried to obtain NiFeMOF / NF.
[0066] Step 2, dissolve 0.05mmol of sodium tungstate in 30mL of a mixed solvent of anhydrous ethanol and deionized water in a volume ratio of 10:20. Immerse the NiFeMOF / NF obtained in step 1 into the mixed liquid. The mixed system is subjected to solvent thermal treatment at 140°C for 6h. The obtained product is washed with anhydrous ethanol and deionized water, and vacuum dried. The obtained material is tungsten-doped nickel-iron hydroxide W-NiFeOH / NF.
[0067] Step 3, placing the W-NiFeOH / NF obtained in step 2 and 1.5 g of sodium hypophosphite in the downstream and upstream of the tube furnace respectively, and keeping them at 400°C for 3 hours at a heating rate of 5°C / min under nitrogen protection to obtain the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst W-NiFeP / NF.
Claims
1. A method for preparing a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst, characterized in that: The steps include: S1, in situ growth of NiFeMOF nanosheet arrays on the surface of nickel foam to obtain NiFeMOF / NF; S2, dissolving sodium tungstate in an ethanol solution to obtain a mixed solution, then immersing NiFeMOF / NF in the mixed solution for solvent thermal treatment, and then washing and drying to obtain tungsten-doped nickel-iron hydroxide; S3, tungsten-doped nickel-iron hydroxide and sodium hypophosphite are heat-treated at 300-400° C. in a nitrogen atmosphere at a ratio of 0.05 mmol: (0.5-1.5) g to obtain a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst.
2. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: S1 obtained NiFeMOF / NF according to the following process: Nickel nitrate, ferric chloride and terephthalic acid were dissolved in a mixed solvent consisting of dimethylacetamide, deionized water and anhydrous ethanol, and the molar ratio of nickel nitrate, ferric chloride and terephthalic acid was 9:1:24 to obtain a mixed system. Nickel foam was impregnated into the mixed system, and the ratio of the upper surface area of the nickel foam to the nickel nitrate was 2 cm 2 : 0.15 mmol, and then a solvothermal reaction was carried out, and the obtained complex was washed and dried in sequence to obtain NiFeMOF / NF.
3. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 2, characterized in that: In the mixed solvent, the volume ratio of dimethylacetamide, deionized water and anhydrous ethanol is 28:1:
1.
4. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: The solvent thermal reaction is carried out at 120-160° C. for 4-8 hours.
5. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: The molar ratio of sodium tungstate in S2 to nickel nitrate in S1 is 1:9, and tungsten-doped nickel-iron hydroxide is obtained.
6. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: The solvent thermal treatment described in S2 is carried out at 120-180° C. for 4-8 hours.
7. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: The volume ratio of anhydrous ethanol to deionized water in the ethanol solution described in S2 is (5-25):(25-5), and the ratio of sodium tungstate to ethanol solution is 0.05mmol:30mL.
8. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: When S3 heats the tungsten-doped nickel-iron hydroxide and sodium hypophosphite, it starts from room temperature and heats to 300-400°C at a heating rate of 1-5°C / min.
9. The method for preparing the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to claim 1, characterized in that: S3: The tungsten-doped nickel-iron hydroxide and sodium hypophosphite are kept at 300-400° C. for 1-3 hours to obtain a MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst.
10. A MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst obtained by the preparation method of the MOF-derived tungsten-doped nickel-iron phosphide bifunctional electrocatalyst according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of nitrogen-doped carbon nanosheet-cobalt-nickel-iron three-transition-metal composite material and application of nitrogen-doped carbon nanosheet-cobalt-nickel-iron three-transition-metal composite
CN119663347A
Preparation method of nitrogen-doped carbon nanosheet@cobalt-nickel-iron transition metal composite material and its application in water electrolysis and hydrogen evolution
CN119663347B
Method for electro-catalytic full-decomposition of seawater by using double-site MOF-based catalyst and application of double-site MOF-based catalyst
CN119776877A
Method and application of dual-site MOF-based catalyst electrocatalytic overall seawater splitting
CN119776877B