Boiling-resistant high-temperature insulation sealant and preparation method thereof

By using hybrid silicone resin and metal elements in the sealant to lower the curing temperature and perform hydrophobic treatment, the problems of moisture absorption and corrosion of traditional glue products are solved, efficient boiling resistance and insulation are achieved, and the scope of its application is expanded.

CN118755449APending Publication Date: 2024-10-11WUHAN DOUBLE BOND NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002202.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional high-temperature resistant inorganic adhesive products easily absorb moisture, leading to a decrease in insulation. Water evaporates at high temperatures to produce bubbles, causing the adhesive layer to loosen or fall off. There are also corrosion problems, which limits its application scope.

Method used

Hybrid silicone resin is used as the main component, and metal elements such as titanium, boron, aluminum, and zirconium are introduced to reduce the curing temperature, and additives and fillers are used for hydrophobic treatment to form a stable -Si-O-Si- structure and improve sealing Glue's boiling resistance and electrical insulation.

Benefits of technology

It achieves a sealant that is neutral, non-corrosive, low-temperature cured, has few bubbles, and has suitable viscosity. It has excellent boiling resistance, temperature resistance and air tightness, and is suitable for a variety of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961899420000011
    Figure BDA0004961899420000011
  • Figure BDA0004961899420000041
    Figure BDA0004961899420000041
  • Figure BDA0004961899420000051
    Figure BDA0004961899420000051
Patent Text Reader

Abstract

The invention provides a boiling-resistant high-temperature insulation sealant and a preparation method thereof, the boiling-resistant high-temperature insulation sealant comprises the following components: hybrid silicon resin, a diluent, an auxiliary agent, a filler and a catalyst, and the hybrid silicon resin can be subjected to condensation reaction under the action of the catalyst; one or more of titanium, boron, aluminum and zirconium are introduced into the hybrid silicon resin structure, and the temperature of condensation reaction can be reduced through the induction effect of titanium, boron, aluminum and zirconium; the sealant has the characteristics of neutrality, no corrosion, low viscosity, low-temperature curing, few bubbles, convenience in use and the like, a cured product of the sealant has the characteristics of excellent water boiling resistance, temperature resistance, electrical insulation, air tightness and the like, and the application range is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high temperature resistant sealants, and in particular to a boiling resistant high temperature insulating sealant and a preparation method thereof. Background Art

[0002] Traditional high-temperature-resistant inorganic adhesive products are mostly silicate and phosphate systems. This type of adhesive product can maintain viscosity at high temperatures, so it is widely used in various industrial fields. However, this type of adhesive product is easy to absorb moisture. The adhesive absorbs moisture in the environment, resulting in a cliff-like drop in its insulation, and the insulation cannot be guaranteed; at the same time, moisture will evaporate rapidly at high temperatures, generating a large amount of steam, which will form bubbles in the adhesive layer, causing the adhesive layer to loosen or fall off. Therefore, traditional high-temperature-resistant inorganic adhesive products have poor performance in terms of water boiling resistance, electrical insulation, air tightness, and operability, and their use is greatly limited. Moreover, this type of adhesive product is usually strongly acidic or alkaline, and the adhesive will corrode the substrate to a certain extent after absorbing moisture. In addition, this type of adhesive also has a series of problems such as slow curing and high curing temperature. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the present invention provides a boiling-resistant high-temperature insulating sealant and a preparation method thereof. The sealant has the characteristics of being neutral and non-corrosive, having low viscosity, being curable at low temperature, having few bubbles and being easy to use. The cured product thereof has the characteristics of excellent boiling-resistant, temperature-resistant, electrical insulating and airtight properties and has a wide range of applications.

[0004] The technical solution adopted to achieve the above-mentioned purpose of the present invention is:

[0005] A boiling-resistant high-temperature insulating sealant, wherein the components and weight percentages of the boiling-resistant high-temperature insulating sealant are:

[0006]

[0007] The general structural formula of the hybrid silicone resin is:

[0008] (R 2 3SiO 1 / 2 ) a (R 2 2SiO 2 / 2 ) b (R 2 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 1 SiO 3 / 2 ) e (R 1 2SiO 2 / 2 ) f (R1 3SiO 1 / 2 ) g (XO 3 / 2 ) h (YO 4 / 2 ) i ;

[0009] Wherein a, b, c, d, e, f, g, h, i are all ≥ 0, a+b+c+d+e+f+g+h+i=1;

[0010] R 1 is one or a combination of two or more of hydroxyl, methoxy, ethoxy, propoxy, and isopropoxy, R 1 The group can undergo condensation reaction under the action of catalyst, that is, dehydration condensation between Si-OH and Si-OH and dealcoholization condensation between Si-OH and Si-alkoxy bonds; R 2 It is one or more of methyl, ethyl, propyl, isopropyl, and phenyl; X, Y is one or more of aluminum, titanium, boron, and zirconium, that is, the hybrid silicone resin in this application is one or more of silicon-titanium hybrid silicone resin, silicon-zirconium hybrid silicone resin, silicon-aluminum hybrid silicone resin, and silicon-boron hybrid silicone resin. The inductive effect of aluminum, titanium, boron, and zirconium can reduce the reaction temperature of dehydration condensation between Si-OH and Si-OH and dealcohol condensation between Si-OH and Si-alkoxy bonds, so that the sealant can be cured in a lower temperature range, usually 25-150°C.

[0011] In the general structural formula of the hybrid silicone resin, h+i=0.01~0.30. This is because a high value of h+i generally causes the hybrid silicone resin to cure too quickly and the resin to gel easily; e+f+g=0.03~0.60. This is because the value directly reflects the reaction activity of the hybrid silicone resin. If the value is too low, the moisture curing properties of the resin will be weakened. If the value is too high, the temperature resistance and thermal curing properties of the sealant will be affected; d=0~0.5. The d value will affect the reaction speed and the state after curing of the hybrid silicone resin, but this structure is not a structure that the hybrid silicone resin must have. The hybrid silicone resin may or may not contain this structure. According to different needs, the curing speed of the resin is adjusted by adjusting the d value. Generally, the larger the value of d, the faster the curing speed, but it will not be higher than 0.5, otherwise the resin will easily gel.

[0012] The diluent is one or two or more of methanol, ethanol, isopropanol, n-butanol, butanone, ethyl acetate, n-hexane, cyclohexane, 3-methoxy-3-methylbutanol, dipropylene glycol methyl ether, dipropylene glycol methyl ether acetate, tripropylene glycol methyl ether, and glycerol acetone acetal.

[0013] The auxiliary agent is one or two or more of methyltrimethoxysilane, vinyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. The auxiliary agent absorbs moisture in the air and then hydrolyzes, and then undergoes a condensation reaction with the groups in the silicon hybrid resin, thereby improving the stability and adhesion of the sealant and accelerating the low-temperature moisture curing speed of the sealant.

[0014] The catalyst is one or two or more of an organic tin catalyst, an organic titanium catalyst, and an organic bismuth catalyst; the catalyst is preferably an organic tin catalyst and an organic titanium catalyst, such as dibutyltin dilaurate, dioctyltin dilaurate, tetrabutyl titanate, tetraisopropyl titanate, etc.

[0015] The filler is composed of one or two or more of silicon micropowder, diatomaceous earth, aluminum oxide, magnesium oxide, zinc oxide, silicon carbide, aluminum nitride and boron nitride.

[0016] The filler is hydrophobically treated by a silane coupling agent, or polysiloxane, or a silane coupling agent / stearic acid compound. After the treatment, the microscopic surface hydroxyl groups of the filler are reduced, and the alkoxy or other organic groups are increased, so that the filler can also undergo a hydrolysis condensation reaction with the hybrid silicone resin to form a chemical bond.

[0017] The present invention also provides a method for preparing a boiling-resistant high-temperature insulating sealant, comprising the following steps: (1) pretreatment of raw materials: the filler is fully dehydrated in a drying device set at a temperature of 100-120° C., and the filler is cooled to room temperature and then prepared for use;

[0018] (2) Preparation of sealant: according to the ratio, the hybrid silicone resin, diluent and auxiliary agent are put into the reactor in sequence; under the protection of nitrogen, after repeated mixing, fillers are added according to the ratio, and fully mixed under the protection of nitrogen. Finally, the catalyst is added under the protection of nitrogen. After mixing, it can be filtered and packaged.

[0019] Compared with the prior art, the water boiling resistant high temperature insulating sealant provided by the present invention has the following advantages:

[0020] (1) The formula of the water-boiling high-temperature insulating sealant provided by the present invention is a hybrid silicone resin, a diluent, an auxiliary agent, a filler and a catalyst, wherein the main reactive group of the hybrid silicone resin is Si-R 1 , R 1It is one or a combination of two or more of hydroxyl, methoxy, ethoxy, propoxy, and isopropoxy. Therefore, the hybrid silicone resin can undergo a condensation reaction in the presence of a catalyst (organotin or / and an organic titanium catalyst), that is, dehydration condensation between Si-OH and Si-OH and dealcoholization condensation between Si-OH and Si-alkoxy bonds; at the same time, one or more of titanium, boron, aluminum, and zirconium are introduced into the structure of the hybrid silicone resin, and its induction effect can reduce the reaction temperature of dehydration condensation between Si-OH and Si-OH and dealcoholization condensation between Si-OH and Si-alkoxy bonds, and the curing temperature is low (the curing temperature is from room temperature to 150°C);

[0021] The auxiliary agent in the present invention is methyltrimethoxysilane, vinyltrimethoxysilane or amino-containing methoxysilane. The auxiliary agent absorbs moisture in the air and then hydrolyzes, and then undergoes a condensation reaction with the groups in the silicon hybrid resin, thereby improving the stability and adhesion of the sealant and accelerating the low-temperature moisture curing speed of the sealant.

[0022] In the present invention, the filler is hydrophobically treated by a silane coupling agent, or polysiloxane, or a silane coupling agent / stearic acid compound. After the treatment, the microscopic surface hydroxyl groups of the filler are reduced, and the alkoxy or other organic groups are increased, so that the filler can also undergo a hydrolysis condensation reaction with the hybrid silicone resin to form a chemical bond, thereby improving the stability of the sealant.

[0023] The realization of the curing reaction of the sealant in the present invention depends on the moisture curing and heat curing properties of the hybrid silicone resin. After the hybrid silicone resin is cured, a stable -Si-O-Si- structure is formed, which plays the role of bonding fillers, so that a hard solid like ceramic can be formed. Because the cured product has a high degree of crosslinking and contains a certain amount of organic groups, and the fillers are also subjected to a specific surface treatment, the cured product has good hydrophobicity and water boiling resistance. After high temperature (generally above 600°C), the organic groups are cracked, but the residual -Si-O-Si- structure maintains the original form, so the cured form will not change significantly, and the hard solid form is maintained, and its water boiling resistance is still maintained. The conventional silicate or phosphate system inorganic glue, its curing depends on the high temperature dehydration reaction of silicate or phosphate, and the cured product is boiled after it is fully cured. Because its main components, silicate or phosphate, absorb water and deliquescence, the structure of the cured product is loose or loose after water boiling, and the form cannot be maintained. At the same time, a large number of ions are ionized, and the insulation property is sharply reduced.

[0024] (2) In the present invention, by adjusting the R 1 The type and molar content of the group as well as the type and amount of the catalyst can be used to widely adjust the surface drying time and curing speed of the sealant to meet the needs of different sealant usage scenarios and ensure the operability and convenience of the sealant in actual production and construction.

[0025] (3) The preparation method of the sealant in the present invention is simple, the process conditions are mild, and no additional curing agent or adhesive is required. The prepared water boiling resistant high temperature insulating sealant product is a micro-flowing to flowing fluid, the colloid is fine, the viscosity is 1000-20000mPas, the surface drying time is 1-15min, the specific gravity is ≥2.0, the heat resistance temperature of the cured product is ≥1000℃, the hardness is ≥Shore D50, and the thermal expansion coefficient is ≤90*10 -6 / ℃, thermal conductivity ≥0.6W / m·k, volume resistivity ≥2×10 10 Ω·cm, sleeve compression shear strength ≥1.5MPa, contact angle ≥100°, good resistance to boiling, acid and alkali, and solvents. This sealant is suitable for various sensor potting, heater sealing, component fixation near heat source, heat-resistant molding materials and anti-corrosion coatings, and has great development potential. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0027] The preparation method of the water-boiling-resistant high-temperature insulating sealant of the present invention comprises the following steps: (1) pretreatment of raw materials: the filler is fully dehydrated in a drying device set at a temperature of 100-120° C., and the filler is cooled to room temperature and then prepared for use;

[0028] (2) Preparation of sealant: according to the ratio, the hybrid silicone resin, diluent and auxiliary agent are put into the reactor in sequence; under the protection of nitrogen, after repeated mixing, fillers are added according to the ratio, and fully mixed under the protection of nitrogen. Finally, the catalyst is added under the protection of nitrogen. After mixing, it can be filtered and packaged.

[0029] Example 1

[0030] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0031]

[0032] The hybrid silicone resin 1 has a viscosity of 60 mPa·s (25°C) and is a colorless transparent liquid. Its general structural formula is as follows:

[0033] ((CH3)3SiO 1 / 2 ) 0.05 (C6H5SiO 3 / 2 ) 0.05 (SiO 4 / 2 ) 0.30 (CH3OSiO 3 / 2 ) 0.30 (HOSiO3 / 2 ) 0.15 (TiO 4 / 2 ) 0.15 ;

[0034] In this embodiment, R 1 Hydroxyl and methoxy.

[0035] The prepared water-boiling high-temperature insulating sealant product is an off-white flowing fluid with fine colloid, viscosity of 8000mPas, surface drying time of 5min, and specific gravity of 2.7. The curing method is to stand at room temperature for 1 hour, keep at 50℃ for 2 hours, and keep at 100℃ for 1 hour. The obtained cured product has a heat resistance temperature of 1200℃, a hardness of 75 Shore D, and a thermal expansion coefficient of 75*10 -7 / ℃, thermal conductivity 2.6W / m·k, volume resistivity 2×10 11 Ω·cm, sleeve compression shear strength 2.0MPa, contact angle 105°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

[0036] The above-mentioned “no abnormality” means that after boiling, acid treatment, alkaline treatment and solvent treatment, the strength and morphology of the cured rubber block do not show obvious attenuation.

[0037] Example 2

[0038] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0039]

[0040] The viscosity of hybrid silicone resin 2 is 45 mPa·s (25°C), and it is a colorless transparent liquid. Its general structural formula is as follows:

[0041] ((CH3)3SiO 1 / 2 ) 0.10 (C6H5SiO 3 / 2 ) 0.05 (SiO 4 / 2 ) 0.25 (CH3OSiO 3 / 2 ) 0.30 (HOSiO 3 / 2 ) 0.20 (BO 3 / 2 ) 0.10 ;

[0042] In this embodiment, R 1 Hydroxyl and methoxy.

[0043] The prepared water-boiling high-temperature insulating sealant product is a grayish white flowing fluid with fine colloid, a viscosity of 4500mPas, a surface drying time of 3min, and a specific gravity of 2.6. The curing method is to stand at room temperature for 1 hour, keep warm at 50℃ for 4 hours, and keep warm at 100℃ for 1 hour. The obtained cured product has a heat-resistant temperature of 1250℃, a hardness of 70, and a thermal expansion coefficient of 90*10 -7 / ℃, thermal conductivity 2.45W / m·k, volume resistivity 1×10 11 Ω·cm, sleeve compression shear strength 2.5MPa, contact angle 108°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

[0044] Example 3

[0045] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0046]

[0047]

[0048] The prepared water-boiling high-temperature insulating sealant product is a grayish-white flowing fluid with fine colloid, a viscosity of 3700mPas, a surface drying time of 8min, and a specific gravity of 1.67. The curing method is to stand at room temperature for 0.5 hours, keep warm at 50℃ for 1 hour, and keep warm at 100℃ for 1 hour. The obtained cured product has a heat-resistant temperature of 1050℃, a hardness of 55, and a thermal expansion coefficient of 60*10 -6 / ℃, thermal conductivity 0.75W / m·k, volume resistivity 1×10 10 Ω·cm, sleeve compression shear strength 1.75MPa, contact angle 103°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

[0049] Example 4

[0050] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0051]

[0052] The viscosity of hybrid silicone resin 3 is 28mPa·s (25°C), and it is a colorless transparent liquid. Its general structural formula is as follows:

[0053] ((CH3)3SiO 1 / 2 ) 0.05 (CH3SiO 3 / 2 ) 0.10 (SiO 4 / 2 ) 0.05 (CH3OSiO 3 / 2 ) 0.30 ((CH3O)2SiO 2 / 2 ) 0.15 (HOSiO 3 / 2 ) 0.15 (BO 3 / 2 ) 0.20 ;

[0054] In this embodiment, R 1 Methoxy and hydroxyl.

[0055] The prepared water-boiling high-temperature insulating sealant product is a grayish-white flowing fluid with fine colloid, a viscosity of 3000mPas, a surface drying time of 15min, and a specific gravity of 2.65. The curing method is to stand at room temperature for 1 hour, keep at 50℃ for 4 hours, and keep at 100℃ for 1 hour. The obtained cured product has a heat-resistant temperature of 1300℃, a hardness of 65, and a thermal expansion coefficient of 90*10 -7 / ℃, thermal conductivity 2.5W / m·k, volume resistivity 1×10 11 Ω·cm, sleeve compression shear strength 2.2MPa, contact angle 107°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

[0056] Example 5

[0057] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0058]

[0059] The viscosity of hybrid silicone resin 4 is 92 mPa·s (25°C), and it is a light yellow transparent liquid. Its general structural formula is as follows:

[0060] ((CH3)3SiO 1 / 2 ) 0.10 (CH3SiO 3 / 2 ) 0.10 (SiO 4 / 2 ) 0.45 (C2H5OSiO 3 / 2 ) 0.10((C2H5O)2SiO 2 / 2 ) 0.10 (BO 3 / 2 ) 0.15 ;

[0061] In this embodiment, R 1 It is ethoxy.

[0062] The prepared water-boiling high-temperature insulating sealant product is a grayish-white flowing fluid with fine colloid, a viscosity of 12000mPas, a surface drying time of 2min, and a specific gravity of 2.67. The curing method is to stand at room temperature for 1 hour, keep at 50℃ for 2 hours, and keep at 100℃ for 1 hour. The obtained cured product has a heat-resistant temperature of 1450℃, a hardness of 80, and a thermal expansion coefficient of 75*10 -7 / ℃, thermal conductivity 2.62W / m·k, volume resistivity 1.3×10 11 Ω·cm, sleeve compression shear strength 2.6MPa, contact angle 110°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

[0063] Example 6

[0064] The components and weight percentages of the water boiling resistant high temperature insulating sealant prepared in this embodiment are as follows:

[0065]

[0066] The viscosity of hybrid silicone resin 5 is 18 mPa·s (25°C), and it is a light yellow transparent liquid. Its general structural formula is as follows:

[0067] ((CH3)3SiO 1 / 2 ) 0.10 (CH3SiO 3 / 2 ) 0.10 (C2H5OSiO 3 / 2 ) 0.30 ((C2H5O)2SiO 2 / 2 ) 0.25 (BO 3 / 2 ) 0.25 ;

[0068] In this embodiment, R 1 It is ethoxy.

[0069] The prepared water-boiling high-temperature insulating sealant product is a grayish white flowing fluid with fine colloid, a viscosity of 1900mPas, a surface drying time of 7min, and a specific gravity of 2.65. The curing method is to stand at room temperature for 2 hours, keep at 50℃ for 6 hours, and keep at 100℃ for 1 hour. The obtained cured product has a heat-resistant temperature of 1150℃, a hardness of 67, and a thermal expansion coefficient of 92*10 -7 / ℃, thermal conductivity 2.39W / m·k, volume resistivity 1.1×10 11 Ω·cm, sleeve compression shear strength 2.1MPa, contact angle 107°, medium resistance: no abnormality in water boiling (boiling for 8 hours), no abnormality in acid resistance (25℃, 5% hydrochloric acid aqueous solution, 24h), no abnormality in alkali resistance (25℃, 5% sodium hydroxide aqueous solution, 24h), no abnormality in solvent resistance (25℃, ethyl acetate / alcohol / xylene, 24h).

Claims

1. A high temperature insulating sealant resistant to boiling water, characterized by: The components and weight percentages of the boiling-resistant high-temperature insulating sealant are as follows: The general structural formula of the hybrid silicone resin is: (R 2 3SiO 1 / 2 ) a (R 2 2SiO 2 / 2 ) b (R 2 SiO 3 / 2 ) c (SiO 4 / 2 ) d (R 1 SiO 3 / 2 ) e (R 1 2SiO 2 / 2 ) f (R 1 3SiO 1 / 2 ) g (XO 3 / 2 ) h (YO 4 / 2 ) i ; Where a, b, c, d, e, f, g, h, i are all ≥ 0, a+b+c+d+e+f+g+h+i=1; R 1 is one or a combination of two or more of hydroxy, methoxy, ethoxy, propoxy and isopropoxy; R 2 It is one or a combination of two or more selected from methyl, ethyl, propyl, isopropyl and phenyl; X, Y are one or a combination of two or more selected from aluminum, titanium, boron and zirconium.

2. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: In the general structural formula of the hybrid silicone resin, h+i=0.01-0.30, e+f+g=0.03-0.60, and d=0-0.

5.

3. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: The diluent is one or two or more of methanol, ethanol, isopropanol, n-butanol, butanone, ethyl acetate, n-hexane, cyclohexane, 3-methoxy-3-methylbutanol, dipropylene glycol methyl ether, dipropylene glycol methyl ether acetate, tripropylene glycol methyl ether, and glycerol acetone acetal.

4. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: The auxiliary agent is one or two or more of methyltrimethoxysilane, vinyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

5. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: The catalyst is one or two or more of an organic tin catalyst, an organic titanium catalyst and an organic bismuth catalyst.

6. The boiling-resistant high-temperature insulating sealant according to claim 5, characterized in that: The catalyst is an organic tin catalyst and an organic titanium catalyst.

7. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: The filler is composed of one or two or more of silicon micropowder, diatomaceous earth, aluminum oxide, magnesium oxide, zinc oxide, silicon carbide, aluminum nitride and boron nitride.

8. The boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that: The filler is treated to be hydrophobic by using a silane coupling agent, or polysiloxane, or a silane coupling agent / stearic acid compound composite.

9. A method for preparing the boiling-resistant high-temperature insulating sealant according to claim 1, characterized in that The method comprises the following steps: (1) pretreatment of raw materials: the filler is fully dehydrated in a drying device set at a temperature of 100-120° C., and the filler is cooled to room temperature and then prepared for use; (2) Preparation of sealant: according to the ratio, the hybrid silicone resin, diluent and additive are put into the reaction kettle in sequence; Under nitrogen protection, mix repeatedly and evenly, then add filler according to the ratio, mix thoroughly and evenly under nitrogen protection, and finally add catalyst under nitrogen protection, mix evenly and filter and package.