High-crack-resistance concrete structure in high-altitude low-humidity environment and preparation method of high-crack-resistance concrete structure

By using a composite structure of high-ductility concrete outer layer, frozen concrete middle layer and ordinary concrete inner layer in concrete structures at high altitudes, combined with fiber-reinforced cement-based composite materials, the problem of easy cracking of concrete in high-altitude areas is solved, and construction is reduced. Cost and improved crack resistance, suitable for high cold environments.

CN118769387AActive Publication Date: 2024-10-15SICHUAN UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411007150.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The low humidity, large temperature difference and strong radiation environment in high-altitude areas make concrete structures prone to cracking. Existing anti-cracking measures are costly and difficult to apply across the entire section, and are difficult to effectively resist freezing, thawing and temperature deformation.

Method used

It adopts a high-altitude, low-humidity environment and high crack-resistant concrete structure. The outer layer is high-ductility concrete, the middle layer is frozen concrete, and the inner layer is fluid ordinary concrete. Through freezing treatment and fiber-reinforced cement-based composite materials, a dense micro-crack control network is formed. , reduce construction costs and improve crack resistance.

Benefits of technology

It significantly reduces the construction cost, improves the crack resistance and durability of concrete, avoids frequent maintenance and crack problems, can resist freeze-thaw and large temperature difference deformation, reduces the width and number of cracks, and extends the service life of the structure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-crack-resistance concrete structure in a high-altitude low-humidity environment and a preparation method of the high-crack-resistance concrete structure, and belongs to the technical field of civil engineering. The frozen concrete technology is utilized, and a novel concrete structural form is provided, namely, high-ductility concrete is poured on the outer layer of frozen concrete, and normal-flow-state common concrete is poured on the inner layer of the frozen concrete. According to the structural form, only the range of the protective layer is the high-ductility concrete, and the interior of the protective layer is still the common concrete, so that the effect of remarkably reducing the construction cost is achieved, the engineering problem that the high-ductility concrete cannot be used in a full-section mode due to too high cost is solved, and the technical effect that the outer side concrete is high in crack resistance is achieved. The technology has the effect of performing combined pouring on different types of concrete, mutual hydration is performed, and the durability problem induced by different concrete interfaces is not generated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of civil engineering, and in particular relates to a high-crack-resistant concrete structure for a high-altitude and low-humidity environment and a preparation method thereof. Background Art

[0002] my country has complex geographical conditions. Some areas, such as western Sichuan, are generally at high altitudes and have poor climatic conditions, accompanied by low humidity, large temperature differences, etc. The environmental conditions are severe and not conducive to the molding and development of concrete. The concrete structure cast under these environmental conditions has serious cracking, which is not conducive to its long-term durability and safety development, and may induce huge losses in social and economic benefits.

[0003] Low humidity, large temperature difference and strong radiation in high altitude areas are the main reasons for the widespread cracking of concrete in this special environment. In a low humidity environment, the internal hydration of concrete causes the relative humidity in its pores to drop rapidly, and the pore tensile stress is large, resulting in large self-shrinkage deformation of concrete, which causes cracks. Secondly, when concrete is in a low temperature environment below -5 to -6°C for a long time, the pore water in its cement stone structure will freeze and cause volume expansion, generating expansion stress and osmotic pressure in the internal microstructure of concrete, further leading to the generation and development of microcracks and causing freeze-thaw cracking of the concrete structure. At the same time, under the environment of hydration heat effect, solar radiation and large temperature difference, the temperature stress of concrete is also large, and some temperature cracks will also occur. Once the concrete structure has serious cracking, it will have a great impact on the durability of the entire structure and the safety during use.

[0004] To address the cracking problem of concrete structures in high-altitude cold regions, the current common methods include optimizing the concrete mix ratio, surface thermal insulation and moisture retention, etc. However, for the construction of concrete structures in high-altitude areas, the altitude is high, the construction conditions are harsh, and the construction equipment and materials are inconvenient to transport. Many anti-cracking measures are difficult to implement effectively. The current method commonly used on construction sites is to strengthen the maintenance of concrete and extend the wet maintenance time to ensure that the concrete is fully hydrated and improve its crack resistance. However, in the special environment of high-altitude areas, once the maintenance measures are removed, cracking caused by environmental impacts will occur immediately. This method can only treat the symptoms but not the root cause. The main reason is that the tensile strength of the concrete itself is too low to withstand such a special environment.

[0005] In response to the above cracking problem, there is currently a high-ductility concrete, which is a fiber-reinforced cement-based composite material. Compared with traditional concrete, it is characterized by high ductility and strong crack width control ability. A large number of fine high elastic modulus fibers are added to the high-ductility concrete. These fibers are evenly distributed in the cement matrix to form a dense micro-crack control network, which can effectively prevent the generation and development of cracks and improve the overall toughness and crack resistance of the material. The use of this type of concrete can effectively reduce the cracking problem of concrete structures in high-altitude cold areas. However, the cost of high-ductility concrete is too high and it does not meet the conditions for full-section application of concrete structures. Summary of the invention

[0006] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a highly crack-resistant concrete structure for a high-altitude and low-humidity environment and a preparation method thereof, so as to solve the technical problem that the existing concrete structure is prone to cracking under special environments.

[0007] The technical solution of the present invention to solve the above technical problems is as follows: a high crack-resistant concrete structure for a high-altitude and low-humidity environment is provided, characterized in that the outer layer of the high crack-resistant concrete structure is high-ductility concrete, the middle layer is frozen concrete, and the inner layer is fluid ordinary concrete.

[0008] Furthermore, the thickness of high ductility concrete is 20-50 mm; the thickness of frozen concrete is 80-120 mm.

[0009] Furthermore, the thickness of the high ductility concrete is 30 mm; and the thickness of the frozen concrete is 100 mm.

[0010] Furthermore, high ductility concrete is a fiber-reinforced cementitious composite material.

[0011] Furthermore, the fiber in the fiber-reinforced cement-based composite material is at least one of steel fiber and polyvinyl alcohol fiber.

[0012] The present invention also provides a method for preparing a high-crack-resistant concrete structure in a high-altitude and low-humidity environment, comprising the following steps:

[0013] (1) freezing ordinary concrete to obtain frozen concrete, which is then fixed to a steel cage;

[0014] (2) The outer layer of the frozen concrete prepared in step (1) is poured with high-ductility concrete, and the inner layer is poured with fluid ordinary concrete.

[0015] Furthermore, in step (2), during the pouring process, the heights of the outer layer of high-ductility concrete and the inner layer of fluid-state ordinary concrete are kept consistent.

[0016] The present invention has the following beneficial effects:

[0017] (1) The present invention proposes to use frozen concrete technology to propose a new type of concrete structure, that is, high-ductility concrete is poured on the outer layer of frozen ordinary concrete, and ordinary concrete with normal flow state is poured on the inner layer of frozen ordinary concrete. This structure only has high-ductility concrete within the protective layer, and the interior is still ordinary concrete. This has the effect of significantly reducing construction costs, solving the engineering problem that high-ductility concrete cannot be used in full section due to its high cost, and achieving the technical effect of high crack resistance of the outer concrete. This technology has the effect of combining and pouring different types of concrete, and they are mutually hydrated, and will not cause durability problems induced by different concrete interfaces.

[0018] (2) Frozen concrete is not only the structural concrete of the column itself, but also serves as a barrier to isolate the outer high-ductility concrete from entering the ordinary concrete. It also has the function of reducing the hydration heat of the outer high-ductility concrete and preventing thermal stress caused by excessive hydration heat. Frozen concrete will melt under the joint action of the inner and outer concrete layers, and at this time it will form an interwoven whole with the inner and outer concretes, so there is no interface that affects strength or durability.

[0019] (3) The outer layer of high-ductility concrete itself has high crack resistance, which can significantly reduce the width of cracks, avoid frequent maintenance when the entire section is ordinary concrete, improve the turnover efficiency of the formwork, reduce the amount of water used for maintenance, and prevent the problem of ordinary concrete easily cracking under special environments such as low humidity and large temperature differences. At the same time, the high-ductility layer concrete has high durability and can resist freeze-thaw, large temperature difference deformation and other problems during service. DETAILED DESCRIPTION

[0020] The following examples are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0021] Example 1

[0022] A high-crack-resistant concrete structure in a high-altitude, low-humidity environment, with an outer layer of high-ductility concrete, a middle layer of frozen concrete, and an inner layer of ordinary concrete in a normal flow state, is prepared by the following method: This embodiment will prepare a cylindrical concrete short column with a diameter of 500mm and a height of 500mm. The thickness of the outer high-ductility concrete protective layer is 30mm. First, a frozen concrete ring with an inner diameter of 240mm, an outer diameter of 440mm, a ring width of 100mm, and a height of 500mm is prepared. P.0 42.5 silicate cement is used. The concrete type is ordinary concrete with a design strength of C30. After pouring, it is directly placed in a liquid nitrogen freezer to absorb heat through the evaporation of liquid nitrogen to produce a cooling effect to experiment the effect of freezing. When the concrete specimen reaches -40°C, it is taken out and placed inside a short column mold. During the process, the center of the ring is ensured to coincide with the center of the cylindrical mold plane. Ordinary concrete with the same proportion as the frozen ring is used for pouring at the center of the interior, and high-ductility concrete is used for pouring at the same time on the exterior. The height inside and outside is kept consistent during the pouring process. Among them, the mix ratio (mass ratio) of ordinary concrete is water: cement: fly ash: water reducer: sand: gravel = 45:100:25:1.25:144:289; the mix ratio (mass ratio) of high ductility concrete is silicate cement P.O42.5: sand: steel fiber: polyvinyl alcohol fiber: water: water reducer: early strength agent = 1400:2800:190:30:530:10:35.

[0023] After demolding, the concrete surface cracks were detected and placed in a laboratory simulation environment with a humidity of 30% and a temperature difference of 30°C between day and night (the daytime period is 7:00-19:00, the temperature is 30°C from 11:00-15:00, and the temperature is 25°C during the rest of the daytime period; the night period is 19:00-7:00 the next day, and the temperature is 0°C) for 28 days of curing. The width and number of cracks in the concrete were evaluated, and the crack positions were determined by visual inspection and the specific width was measured using a crack width gauge. The highly crack-resistant concrete structure prepared in this embodiment showed no visible cracks after testing.

[0024] Example 2

[0025] A high-crack-resistant concrete structure in a high-altitude, low-humidity environment, with an outer layer of high-ductility concrete, a middle layer of frozen concrete, and an inner layer of ordinary concrete in a normal flow state, is prepared by the following method: This embodiment will prepare a 500mm diameter, a 3000mm height, and an outer layer of high-ductility concrete protective layer with a thickness of 50mm. First, a frozen concrete ring with an inner diameter of 200mm, an outer diameter of 400mm, a ring width of 100mm, and a height of 3000mm is prepared, using P.0 42.5 silicate cement, the concrete type is ordinary concrete, and the design strength is C30. After pouring, it is directly placed in a liquid nitrogen freezer to absorb heat through the evaporation of liquid nitrogen, thereby generating a cooling effect to achieve freezing. When the concrete specimen reaches -40°C, it is taken out and placed inside a column mold. During the process, the center of the ring is ensured to coincide with the center of the plane of the column mold. Ordinary concrete with the same proportion as the frozen ring is used for pouring at the center of the interior, and high-ductility concrete is used for pouring at the same time on the exterior. The height inside and outside is kept consistent during the pouring process. Among them, the mix ratio (mass ratio) of ordinary concrete is water: cement: fly ash: water reducer: sand: gravel = 45: 100: 25: 1.25: 144: 289; the mix ratio (mass ratio) of high ductility concrete is silicate cement PO 42.5: sand: steel fiber: polyvinyl alcohol fiber: water: water reducer: early strength agent = 1400: 2800: 190: 30: 530: 10: 35.

[0026] After pouring, the method of covering with soaked geotextile is used for maintenance immediately. During the maintenance period, water is sprinkled 5 times a day, and 8 times in windy weather to ensure that the covering is always kept moist (20% humidity environment). After 7 days of moisturizing maintenance, the mold is removed and then naturally cured to 28 days of age. Then the high crack-resistant concrete structure prepared in this embodiment is placed in an actual high-altitude and low-humidity environment for surface crack detection (the detection method is the same as in Example 1). The specific detection address is Meigu County, Sichuan Province. The local geographical location is relatively remote, the altitude is high, the environmental conditions are relatively harsh, the humidity is low, and the temperature difference between day and night is large. The test results are: the high crack-resistant concrete structure prepared in this embodiment has no visible cracks after testing. This embodiment and Example 1 better illustrate that the concrete pouring using a new structural form can effectively avoid cracking of the concrete structure.

[0027] Comparative Example 1: Ordinary concrete

[0028] Comparative Example 1: A concrete short column with a diameter of 500 mm and a height of 500 mm was prepared. The cement selected was silicate cement PO 42.5, the concrete type was ordinary concrete, and the design strength was C30. The proportion (mass ratio) of the ordinary concrete was water: cement: fly ash: water reducing agent: sand: gravel = 45:100:25:1.25:144:289.

[0029] After the prepared concrete slurry was poured into the test mold, it was placed in a laboratory simulated environment with a humidity of 80% and a temperature of 20°C for 28 days of curing. After the mold was removed, the concrete surface cracks were detected (the detection method was the same as in Example 1). After the test, the result was: the concrete structure surface prepared in Comparative Example 1 had no cracks. The results of this comparative example show that under normal curing conditions, the concrete will not have visible cracks after the mold is removed.

[0030] Comparative Example 2: Ordinary Concrete

[0031] Comparative Example 2: A concrete short column with a diameter of 500 mm and a height of 500 mm was prepared. The cement selected was silicate cement PO 42.5, the concrete type was ordinary concrete, and the design strength was C30. The proportion (mass ratio) of the ordinary concrete was water: cement: fly ash: water reducing agent: sand: gravel = 45:100:25:1.25:144:289.

[0032] After the prepared concrete slurry is poured into the test mold, it is placed in a laboratory simulation environment with a humidity of 30% and a temperature difference of 30°C between day and night (the daytime period is 7:00-19:00, the temperature is 30°C between 11:00-15:00, and the temperature is 25°C during the rest of the daytime period; the night period is 19:00-7:00 the next day, and the temperature is 0°C) for 28 days of curing. After demolding, the concrete surface cracks are detected (the detection method is the same as that of Example 1). After testing, the results are as follows: the concrete structure prepared in Comparative Example 2 has obvious cracks, the number of cracks with a length greater than 1 mm is 7, the longest crack length is 15 mm, and the maximum crack width is 0.45 mm.

[0033] The maintenance environment of this comparative example simulates the climatic conditions of the high-altitude cold areas of Tibet. The maximum temperature during the day is about 30°C, which drops to 0°C at night, accompanied by long periods of sunshine. The average humidity is 30%. Compared with Comparative Example 1, it is found that this specimen has obvious cracking after demolding. The reason is that under the low-humidity maintenance conditions, the surface moisture of the concrete is lost quickly, and shrinkage cracks appear; at the same time, under the conditions of large temperature difference, the temperature drops quickly, and temperature cracks appear. The maintenance environment of Example 1 also simulates the high-altitude cold areas. Compared with Comparative Example 2, it is found that under the same low-humidity and large temperature difference maintenance conditions, when using a new type of concrete structure, no cracks visible to the naked eye will appear. Even if there are cracks, the crack width is within the crack width value allowed by our country's standards.

[0034] In summary, the concrete with the novel structure of the present invention can reduce the cracking problem of concrete in high-altitude cold areas.

[0035] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A highly crack-resistant concrete structure for high altitude and low humidity environments, characterized in that: The outer layer of the high crack resistance concrete structure is high ductility concrete, the middle layer is frozen concrete, and the inner layer is fluid concrete.

2. The high-crack-resistant concrete structure for high-altitude and low-humidity environments according to claim 1 is characterized in that: The thickness of the high-ductility concrete is 20-50 mm; the thickness of the frozen concrete is 80-120 mm.

3. The high-crack-resistant concrete structure for high-altitude and low-humidity environments according to claim 2 is characterized in that: The thickness of the high-ductility concrete is 30 mm; the thickness of the frozen concrete is 100 mm.

4. The high-crack-resistant concrete structure for high-altitude and low-humidity environments according to claim 1 is characterized in that: The high ductility concrete is a fiber-reinforced cement-based composite material.

5. The highly crack-resistant concrete structure according to claim 4, characterized in that: The fiber in the fiber-reinforced cement-based composite material is at least one of steel fiber and polyvinyl alcohol fiber.

6. The method for preparing a high-crack-resistant concrete structure in a high-altitude, low-humidity environment according to any one of claims 1 to 5, comprising the following steps: (1) freezing the fluid concrete to obtain frozen concrete, which is then fixed to the steel cage; (2) The outer layer of the frozen concrete prepared in step (1) is poured with high ductility concrete, and the inner layer is poured with fluid concrete.

7. The preparation method according to claim 6, characterized in that: In the step (2), during the pouring process, the heights of the outer layer high ductility concrete and the inner layer fluid dynamic concrete are kept consistent.

Citation Information

Patent Citations

  • Mining concrete refrigerating machine

    CN104315781A

  • Construction method of piled anchor and liquid nitrogen frozen earth wall combined support system

    CN108797601A

  • Preparation process of high-altitude region saline-alkali resistant concrete

    CN109734394A

  • Winter application micro-expansive concrete and preparation method thereof

    CN114716208A

  • Pouring method of high-crack-resistance fiber concrete composite material

    CN117532714A