Modified polysiloxane hybrid silicone hydrogel contact lens and preparation method thereof

By modifying the polyorganosiloxane hybrid silicone hydrogel material, the insufficient mechanical properties and biocompatibility problems caused by the increased oxygen permeability and water absorption of contact lens materials are solved, achieving high light transmittance and good mechanics. High-performance silicone hydrogel contact lenses for contact lenses and other medical materials.

CN118772344APending Publication Date: 2024-10-15JIANGSU DUOZI MEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410878017.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

When improving oxygen permeability and water absorption, existing contact lens materials have insufficient mechanical properties and biocompatibility, and are prone to inflammation, making it difficult to meet the needs for comfort and safety.

Method used

Modified polyorganosiloxane hybrid silicone hydrogel material is used, and through a combination of specific components and initiators, silicone hydrogel contact lenses with high oxygen permeability, hydrophilicity and good mechanical properties are prepared. Plasma irradiation and photoinitiated polymerization processes form a three-dimensional molecular network.

Benefits of technology

Silicone hydrogel contact lenses that achieve high light transmittance, good mechanical properties and biocompatibility are suitable for contact lenses and other medical materials, improving comfort and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772344A_ABST
    Figure CN118772344A_ABST
Patent Text Reader

Abstract

The invention discloses a modified polysiloxane hybrid silicone hydrogel contact lens and a preparation method thereof, and belongs to the field of new material synthesis. The contact lens is made of a silicone hydrogel material prepared by taking a mixed monomer solution of modified polysiloxane and acrylic acid or acrylic ester or vinyl pyrrolidone as a raw material solution. The contact lens has good air permeability and light transmittance, and excellent hydrophilicity and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of contact lenses (corneal contact lenses) and organosilicon hybrid hydrogel materials, and relates to a modified polyorganosiloxane hybrid silicone hydrogel contact lens, in particular to a contact lens produced by a mixed monomer solution prepared with modified polyorganosiloxane. Background Art

[0002] Contact lenses can not only be used to correct vision, but are also widely popular because they are concealed to wear and can be given colors to create the effect of beauty lenses, becoming a fashion among young people.

[0003] Good oxygen permeability and hydrophilicity are two important technical indicators of contact lenses, which can ensure that the eye tissue has a good gas environment and maintain water balance.

[0004] Hydrogel materials with poly(hydroxyethyl methacrylate) as the main body are one of the main materials for manufacturing contact lenses. This material has a strong water absorption capacity, and within a certain range of water absorption, its oxygen permeability will increase with the increase of water absorption capacity, but as the water absorption capacity increases, the mechanical properties of the hydrogel will decrease significantly. At the same time, hydrogels with too strong water absorption capacity will absorb moisture in the eyeball, which will make the wearer feel dry eyes. In addition, after reaching the saturated water absorption rate, the improvement of its oxygen permeability will be limited. Therefore, the comfort of contact lenses produced with hydrogel materials with poly(hydroxyethyl methacrylate) as the main body is always not satisfactory. Improving the oxygen permeability of hydrogel materials has become one of the main directions of contact lens development.

[0005] Bausch and Lomb began selling pure astigmatism in 2004, which was the first silicone hydrogel contact lens. The material used in this contact lens is silicone hydrogel, which is a hybrid material of organic silicon. At present, silicone hydrogel materials are gradually replacing the early hydrogel materials based on poly(hydroxyethyl methacrylate) due to their better oxygen permeability and suitable hydrophilicity, and have become the main material for manufacturing contact lens products. Today, many companies in the world, including Johnson & Johnson, Bausch and Lomb, and Haichang, mainly use organic siloxane mixed with various hydrophilic monomers to produce silicone hydrogel contact lenses.

[0006] The polymethylsiloxane (PDMS) structure is the most common molecular structure in silicone hydrogel contact lenses. The most common method for producing silicone hydrogel contact lenses is to copolymerize PDMS macromonomers with other functional monomers. Introducing the PDMS structure into contact lenses helps the contact lenses to obtain good air permeability, biocompatibility and mechanical properties. However, the introduction of the PDMS structure also brings several inherent defects. First, the hydrophobicity of PDMS will reduce the water absorption rate of contact lenses, thereby reducing the comfort of contact lenses; second, PDMS can easily cause corneal contact lenses to adsorb proteins, contaminate contact lenses and cause inflammation. Therefore, a more reasonable design of silicone hydrogel materials is needed to meet the needs of the contact lens industry. Summary of the invention

[0007] In view of the above problems, the present invention provides a new modified siloxane monomer, and prepares it into a mixed monomer solution to prepare a silicone hydrogel material and a contact lens with a new molecular structure, and provides a method for producing the silicone hydrogel material and the contact lens. The silicone hydrogel of the present invention has excellent oxygen permeability, hydrophilicity and light transmittance, which can well make up for the shortcomings of insufficient hydrophilicity and limited oxygen permeability improvement of the polymethylsiloxane (PDMS) molecular network, and has stable and uniform performance, good mechanical properties and biocompatibility, no toxic side effects, and is conducive to use as contact lenses or other medical materials.

[0008] To achieve the above object, the present invention adopts the following technical solutions:

[0009] A modified polyorganosiloxane hybrid silicon hydrogel contact lens is prepared from a modified polyorganosiloxane hybrid silicon mixed monomer solution, wherein the modified polyorganosiloxane hybrid silicon mixed monomer solution contains a mixed monomer and an initiator;

[0010] The mixed monomer consists of component A and component B, wherein:

[0011] Component A is modified polyorganosiloxane.

[0012] Component B is a mixture of one or more of acrylic acid, acrylic esters and vinyl pyrrolidone;

[0013] Component A accounts for 20% to 80% of the total weight of the mixed monomers, and component B accounts for 80% to 20% of the total weight of the mixed monomers; the total amount of component A and component B is 100%;

[0014] The concentration of the mixed monomer in the modified polyorganosiloxane hybrid silicon mixed monomer solution is 10% to 70%;

[0015] The weight of the initiator is 0.1-10% of the weight of the mixed monomers.

[0016] Further: The preparation method of the modified polyorganosiloxane is to mix the hydroxy silicone oil with a solvent after plasma irradiation, wherein the mass concentration of the hydroxy silicone oil is 20% to 50%; then, methyl methacrylate isocyanate is added at 30 to 40°C, and finally, dibutyltin dilaurate is added to react for 1 to 5 hours, and after the reaction is completed, the reaction is cooled to room temperature, and then distilled at 45 to 50°C to obtain the modified polyorganosiloxane.

[0017] Preferably: the power of plasma irradiation is 1-2KW, the atmosphere is nitrogen, and the irradiation time is 3-10 minutes;

[0018] In the mixture of hydroxy silicone oil and methacrylate isocyanate, n(OH):n(NCO)=1~2:1~2;

[0019] The amount of dibutyltin dilaurate used is 2% to 8% of the mass of methacrylate isocyanate.

[0020] Further: the acrylic acid is at least one of acrylic acid and methacrylic acid;

[0021] The acrylic acid ester monomer is a mixture of one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, ethylene glycol dimethacrylate, polyethylene glycol 600 dimethacrylate, and polyethylene glycol diacrylate;

[0022] Preferably: component B is acrylic acid and acrylic acid ester in a mass ratio of 3-8:20-80, or component B is acrylic acid ester and vinyl pyrrolidone in a mass ratio of 20-70:10-15;

[0023] It is further preferred that: component B is hydroxyethyl methacrylate, methacrylic acid and ethylene glycol dimethacrylate in a mass ratio of 30-80:3-8:3-8;

[0024] or component B is hydroxyethyl methacrylate, methacrylic acid and polyethylene glycol 600 dimethacrylate in a mass ratio of 30-80:3-8:3-8;

[0025] or component B is hydroxyethyl methacrylate, vinyl pyrrolidone and polyethylene glycol 600 dimethacrylate in a mass ratio of 20-80:10-20:3-8;

[0026] Or component B is hydroxyethyl methacrylate, methacrylic acid and polyethylene glycol 600 dimethacrylate in a mass ratio of 10-30:3-8:3-8.

[0027] Further: the solvent is a mixture of one or more of dichloromethane, chloroform, tetrachloromethane, isopropanol, methanol, ethanol, butanol and water.

[0028] Further: the initiator includes a photoinitiator and a thermal initiator.

[0029] Further: the initiator is azobisisoheptanenitrile, azobisisobutyronitrile, benzoyl peroxide, diisopropyl peroxide, ditert-butyl peroxide, diisopropyl peroxydicarbonate, potassium persulfate (CAS No.: 7727-21-1), ammonium persulfate, hydrogen peroxide, hydroperoxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-hydroxy-2-methyl-1-phenyl-1-propanone (CAS No.: 7473-98-5), 1-hydroxycyclohexyl phenyl ketone (CAS No.: 947-19-3), methyl benzoylformate, benzoin dimethyl ether, diphenyl acetone, α-aminoalkyl phenone, dibenzoylphenyl phosphine oxide, benzophenone, diphenyl (2,4,6-trimethylbenzoyl) ) phosphine oxide, 2,2-dimethoxyphenylacetophenone, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-dimethylaminoethyl benzoate, 2-methylbenzophenone, 4-methylbenzophenone, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether mixture, benzoin isobutyl ether, a blend of benzoin n-butyl ether and benzoin isobutyl ether, α,α-diethoxyacetophenone, α,α-di-(n-butoxy)-acetophenone, isopropylthioxanthone, oxalic acid (CAS No. 144-62-7), alcohol, amine, glucose, sodium bisulfite, sodium thiosulfate, thiol, cyclopentaneate, and an organic metal compound.

[0030] Furthermore: the concentration of the mixed monomer in the modified polyorganosiloxane hybrid silicon mixed monomer solution is 40% to 70%.

[0031] Furthermore: the weight of the initiator is 0.1-2% of the weight of the mixed monomers.

[0032] A method for preparing the modified polyorganosiloxane hybrid silicon hydrogel contact lens is provided, wherein the modified polyorganosiloxane hybrid silicon mixed monomer solution is placed in a mold and prepared at -10°C to 100°C by a photo-initiated polymerization or a thermal-initiated polymerization process.

[0033] The processing principle of the contact lenses produced by the modified polyorganosiloxane mixed monomer solution of the present invention is as follows:

[0034] Component A and component B are mixed with solvent and initiator, and polymerization reaction occurs under ultraviolet light or at a certain temperature to form a three-dimensional modified polyorganosiloxane hybrid silicon hydrogel molecular network:

[0035] The structure of the B segment includes III, IV or V:

[0036]

[0037] Where R 1 Selected from H or CH 3 , R 2 Selected from H, CH 3 , CH 2 CH 3 , CH 2 OH, CH 2 CH 2 OH or CH 2 CH 2 CH 2 OH. The value range of I and O is 1 to 90.

[0038] On the other hand, the application scope of the modified polyorganosiloxane mixed monomer solution as described above is not limited to the production of contact lenses, but can also be used to produce other products, such as tissue engineering scaffolds, artificial transplants, medical dressings, artificial skin, etc.

[0039] The beneficial effects of this hair are as follows:

[0040] (1) Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers have high light transmittance, high oxygen permeability and appropriate water absorption.

[0041] (2) Silicone hydrogel contact lenses produced using modified polysiloxane mixed monomers have good mechanical properties.

[0042] (3) Silicone hydrogel contact lenses produced using modified polysiloxane mixed monomers have good biocompatibility and no toxic side effects.

[0043] (4) Silicone hydrogel materials produced using modified polysiloxane mixed monomers have a wide range of applications. In addition to being used in the production of contact lenses, they can also be used in various biological and medical materials, such as artificial cartilage tissue, drug carriers, antibacterial materials, and biosensors, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The appearance of the silicone hydrogel contact lens prepared in Example 1 shows that the contact lens prepared using the formula of Example 1 has a stable shape and is wearable. The appearance of the contact lenses prepared in other examples is similar to Figure 1 There is no significant difference.

[0045] Figure 2 The biocompatibility and cytotoxicity data of the silicone hydrogels prepared in Examples 1-9 indicate that the materials used to prepare silicone hydrogel contact lenses are biocompatible and have no obvious cytotoxicity. DETAILED DESCRIPTION

[0046] The following examples are only used as examples to illustrate the specific embodiments of the present invention, but these examples cannot limit the scope of the present invention.

[0047] Example 1

[0048] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0049] (1) Component A modified polyorganosiloxane, accounting for 20% of the weight of the mixed monomer. The production process of component A is as follows: place hydroxy silicone oil in a vacuum plasma cleaning machine (PTL-VM500, the same below), treat it under plasma at a power of 300W and a nitrogen atmosphere for 3 minutes, and then mix and stir it with dichloromethane. The mass concentration of hydroxy silicone oil is 20%, and the temperature is adjusted to 35°C. Add methyl methacrylate isocyanate, fix n(OH):n(NCO)=1:1, add dibutyltin dilaurate, and the amount of dibutyltin dilaurate is 4% of the mass of methyl methacrylate isocyanate. React for 1 hour, and stop heating after the reaction. After the reaction liquid cools to room temperature, change the device to a distillation device, adjust the water bath temperature to 50°C, and obtain modified polyorganosiloxane after constant temperature distillation.

[0050] Component B is 70% hydroxyethyl methacrylate, 5% methacrylic acid, and 5% ethylene glycol dimethacrylate, based on the weight of the mixed monomers;

[0051] The solvent is isopropanol, and a mixed monomer solution with a mixed monomer mass concentration of 60% is prepared; the initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (D-1173), and the weight is 1% of the mixed monomer weight.

[0052] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0053] (3) The solvent in the silicone hydrogel sample was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, using the Soxhlet extraction method to obtain a silicone hydrogel contact lens (referred to as Sample 1).

[0054] Figure 1 This is a photo of the silicone hydrogel contact lens prepared in Example 1. Figure 1 It can be seen from Table 1 that the silicone hydrogel contact lens synthesized in this example is colorless and transparent in appearance, dimensionally stable, and has a certain mechanical strength.

[0055] Comparative Example 1

[0056] 1. Compared with Example 1, PDMS that has not been plasma-modified is used to replace component A, and the other compositions and molding processes are exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 1).

[0057] 2. Performance testing of the obtained contact lenses

[0058] Table 1. Effects of different monomers on silicone hydrogel contact lenses

[0059]

[0060] Example 2

[0061] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0062] (1) Component A is a modified polyorganosiloxane, prepared in the same manner as in Example 1, and Component A accounts for 60% by weight of the mixed monomers;

[0063] Component B is 30% hydroxyethyl methacrylate, 5% methacrylic acid, and 5% ethylene glycol dimethacrylate by weight of the mixed monomers;

[0064] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0065] The initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (D-1173), and its weight is 1% of the weight of the mixed monomers.

[0066] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0067] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, using the Soxhlet extraction method to obtain a silicone hydrogel contact lens (referred to as Sample 2).

[0068] Sample 2 synthesized in this embodiment is colorless and transparent in appearance, dimensionally stable, and has certain mechanical strength, which is similar to that of Example 1.

[0069] Table 2. Effects of different monomers on silicone hydrogel contact lenses

[0070]

[0071] Example 3

[0072] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0073] (1) Component A modified polyorganosiloxane, accounting for 60% of the weight of the mixed monomer. The production process of component A is as follows: place hydroxy silicone oil in a vacuum plasma cleaning machine (PTL-VM500), treat it for 10 minutes under a power of 300W and a nitrogen plasma atmosphere, and then mix and stir it with dichloromethane. The mass concentration of hydroxy silicone oil is 50%, and the temperature is adjusted to 35°C. Add methyl methacrylate isocyanate, fix n(OH):n(NCO)=1:1, add dibutyltin dilaurate, and the amount of dibutyltin dilaurate is 8% of the mass of methyl methacrylate isocyanate. React for 1 hour, and stop heating after the reaction. After the reaction liquid cools to room temperature, change the device to a distillation device, adjust the water bath temperature to 50°C, and obtain modified polyorganosiloxane after constant temperature distillation.

[0074] Component A accounts for 60% of the weight of the mixed monomers;

[0075] Component B is 30% hydroxyethyl methacrylate, 5% methacrylic acid, and 5% polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0076] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0077] The initiator is 1-hydroxycyclohexyl phenyl ketone, the weight of which is 1% of the weight of the mixed monomers.

[0078] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0079] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, and the elution method was Soxhlet extraction to obtain a silicone hydrogel contact lens (referred to as Sample 3).

[0080] Sample 3 synthesized in this embodiment is colorless and transparent in appearance, dimensionally stable, and has certain mechanical strength, which is similar to that of Example 1.

[0081] Comparative Example 2

[0082] Compared with Example 3, PDMS that has not been plasma-modified was used to replace component A, and other compositions and molding processes were exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 2).

[0083] 2. Performance testing of the obtained contact lenses

[0084] Table 3. Effects of different monomers on silicone hydrogel contact lenses

[0085]

[0086]

[0087] Example 4

[0088] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0089] (1) Component A is a modified polyorganosiloxane, and the preparation method is the same as that of Example 3, and component A accounts for 30% by weight of the mixed monomers;

[0090] Component B is 60% of hydroxyethyl methacrylate, 5% of methacrylic acid, and 5% of polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0091] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0092] The initiator is 1-hydroxycyclohexyl phenyl ketone, the weight of which is 1% of the weight of the mixed monomers.

[0093] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0094] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, using the Soxhlet extraction method to obtain a silicone hydrogel contact lens (referred to as Sample 4).

[0095] Sample 4 synthesized in this embodiment has a colorless and transparent appearance, is dimensionally stable, and has a certain mechanical strength, which is similar to that of Example 1 ( Figure 1 )resemblance.

[0096] Table 4. Effects of different monomers on silicone hydrogel contact lenses

[0097]

[0098] Example 5

[0099] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0100] (1) Component A is a modified polyorganosiloxane, prepared in the same manner as in Example 1, and Component A accounts for 20% by weight of the mixed monomers;

[0101] Component B is 60% of hydroxyethyl methacrylate, 15% of vinyl pyrrolidone, and 5% of polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0102] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0103] The initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (D-1173), and its weight is 1% of the weight of the mixed monomers.

[0104] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0105] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, and the elution method was Soxhlet extraction to obtain a silicone hydrogel contact lens (referred to as Sample 5).

[0106] Sample 5 synthesized according to this embodiment has a colorless and transparent appearance, stable dimensions, and a certain mechanical strength, which is similar to that of Example 1 ( Figure 1 )resemblance.

[0107] Comparative Example 3

[0108] Compared with Example 5, PDMS that has not been plasma-modified was used to replace component A, and other compositions and molding processes were exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 3).

[0109] 2. Performance testing of the obtained contact lenses

[0110] Table 5. Effects of different monomers on silicone hydrogel contact lenses

[0111]

[0112] Example 6

[0113] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0114] (1) Component A is a modified polyorganosiloxane, prepared in the same manner as in Example 1, and Component A accounts for 65% of the weight of the mixed monomers;

[0115] Component B is 20% hydroxyethyl methacrylate, 10% vinyl pyrrolidone, and 5% polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0116] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0117] The initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (D-1173), and its weight is 1% of the weight of the mixed monomers.

[0118] (2) The mixed monomer solution obtained in step (1) was poured into a polypropylene mold and placed in a UV curing box with a wavelength of 395nm-400nm. The mold was 5cm away from the light source and the irradiation power was adjusted to 600mW / cm 2 The light efficiency is 1000W, and the irradiation time is 50 minutes. After the raw material is solidified and formed, it is cooled to room temperature to eliminate the internal thermal stress of the material, and the mold is opened to obtain the silicone hydrogel sample.

[0119] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, using the Soxhlet extraction method to obtain a silicone hydrogel contact lens (referred to as Sample 6).

[0120] Sample 6 synthesized in this embodiment has a colorless and transparent appearance, stable dimensions, and a certain mechanical strength, which is similar to that of Example 1 ( Figure 1 )resemblance.

[0121] Comparative Example 4

[0122] Compared with Example 5, PDMS that has not been plasma-modified was used to replace component A, and other compositions and molding processes were exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 4).

[0123] 2. Performance testing of the obtained contact lenses

[0124] Table 6. Effects of different monomers on silicone hydrogel contact lenses

[0125]

[0126] Example 7

[0127] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0128] (1) Component A is a modified polyorganosiloxane, prepared in the same manner as in Example 1, and Component A accounts for 65% of the weight of the mixed monomers;

[0129] Component B is 20% hydroxyethyl methacrylate, 10% vinyl pyrrolidone, and 5% polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0130] The solvent is isopropanol, and a mixed monomer solution having a mixed monomer concentration of 60% is prepared;

[0131] The initiator is azobisisoheptanonitrile, the weight of which is 0.2% of the weight of the mixed monomers.

[0132] (2) Pour the mixed monomer solution obtained in step (1) into a polypropylene mold, place it in a heat curing box, raise the temperature to 42°C at a rate of 2°C / min, keep the temperature constant for 3 hours, then raise the temperature to 56°C at a rate of 2°C / min, keep the temperature constant for 2 hours, cool it to room temperature, and open the mold to obtain a silicone hydrogel sample.

[0133] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence by Soxhlet extraction to obtain a silicone hydrogel contact lens (referred to as Sample 7).

[0134] Sample 7 synthesized according to this embodiment has a colorless and transparent appearance, is dimensionally stable, and has a certain mechanical strength. Figure 1 )resemblance.

[0135] Comparative Example 5

[0136] Compared with Example 7, PDMS that has not been plasma-modified was used to replace component A, and other compositions and molding processes were exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 5).

[0137] 2. Performance testing of the obtained contact lenses

[0138] Table 7. Effects of different monomers on silicone hydrogel contact lenses

[0139]

[0140] Example 8

[0141] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0142] (1) Component A is a modified polyorganosiloxane, prepared in the same manner as in Example 1, accounting for 65% of the weight of the mixed monomers;

[0143] Component B is 20% hydroxyethyl methacrylate, 10% vinyl pyrrolidone, and 5% polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0144] The solvent is a mixed solvent of isopropanol and water in a mass ratio of 6:4, and a mixed monomer solution with a mixed monomer concentration of 40% is prepared;

[0145] The initiator is potassium persulfate, the weight of which is 0.2% of the weight of the mixed monomers.

[0146] (2) Pour the mixed monomer solution obtained in step (1) into a polypropylene mold, place it in a heat curing box, raise the temperature to 42°C at a rate of 2°C / min, keep the temperature constant for 3 hours, then raise the temperature to 56°C at a rate of 2°C / min, keep the temperature constant for 2 hours, cool it to room temperature, and open the mold to obtain a silicone hydrogel sample.

[0147] (3) The solvent in the product was eluted with 50%, 25% ethanol aqueous solution and distilled water in sequence by Soxhlet extraction to obtain a silicone hydrogel contact lens (referred to as Sample 8).

[0148] Sample 8 synthesized in this embodiment has a colorless and transparent appearance, stable dimensions, and a certain mechanical strength, which is similar to that of Example 1 ( Figure 1 )resemblance.

[0149] 2. Performance testing of the obtained contact lenses

[0150] Table 8. Effects of different monomers on silicone hydrogel contact lenses

[0151]

[0152] Example 9

[0153] 1. Silicone hydrogel contact lenses produced using modified polyorganosiloxane mixed monomers

[0154] (1) Component A is a modified polyorganosiloxane, and the preparation method is the same as that of Example 3, and component A accounts for 70% by weight of the mixed monomers;

[0155] Component B is 20% hydroxypropyl methacrylate (27813-02-1), 5% methacrylic acid, and 5% polyethylene glycol 600 dimethacrylate, based on the weight of the mixed monomers;

[0156] The solvent is a mixed solvent of isopropanol and water in a mass ratio of 4:6, and a mixed monomer solution with a mixed monomer concentration of 40% is prepared;

[0157] The initiator is a mixture of potassium persulfate and oxalic acid in a mass ratio of 2:1, and the weight of the initiator is 0.3% of the weight of the mixed monomers.

[0158] The mixed monomer solution was stored at 4°C until use.

[0159] (2) The mixed monomer solution obtained in step (1) is poured into a polypropylene mold, placed in a heat curing box, heated to 25 degrees at a rate of 2 degrees Celsius per minute, kept at a constant temperature for 3 hours, and the mold is opened to obtain a silicone hydrogel sample.

[0160] (3) The solvent in the product was eluted with 75%, 50%, 25% ethanol aqueous solution and distilled water in sequence, using the Soxhlet extraction method to obtain a silicone hydrogel contact lens (referred to as Sample 9).

[0161] Sample 9 synthesized according to the embodiment has a colorless and transparent appearance, is dimensionally stable, and has a certain mechanical strength. Figure 1 )resemblance.

[0162] Comparative Example 6

[0163] Compared with Example 9, hydroxyethyl methacrylate was used to replace component A, and other compositions and molding processes were exactly the same to prepare a silicone hydrogel contact lens (referred to as comparative sample 6).

[0164] 2. Performance testing of the obtained contact lenses

[0165] Table 9. Effects of different monomers on silicone hydrogel contact lenses

[0166]

Claims

1. A modified polyorganosiloxane hybrid silicone hydrogel contact lens, Features: It is prepared from a modified polyorganosiloxane hybrid silicon mixed monomer solution, wherein the modified polyorganosiloxane hybrid silicon mixed monomer solution contains a mixed monomer and an initiator; The mixed monomer consists of component A and component B, wherein: Component A is modified polyorganosiloxane. Component B is a mixture of one or more of acrylic acid, acrylic esters and vinyl pyrrolidone; Component A accounts for 20% to 80% of the total weight of the mixed monomers, and component B accounts for 80% to 20% of the total weight of the mixed monomers; the total amount of component A and component B is 100%; The concentration of the mixed monomer in the modified polyorganosiloxane hybrid silicon mixed monomer solution is 10% to 70%; The weight of the initiator is 0.1-10% of the weight of the mixed monomers.

2. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The preparation method of the modified polyorganosiloxane is to mix the hydroxy silicone oil with a solvent after plasma irradiation, wherein the mass concentration of the hydroxy silicone oil is 20% to 50%; then, methyl methacrylate isocyanate is added at 30 to 40° C., and finally, dibutyltin dilaurate is added to react for 1 to 5 hours, and after the reaction is completed, the modified polyorganosiloxane is obtained by cooling to room temperature and then distilling at 45 to 50° C. Preferably: the power of plasma irradiation is 1-2KW, the atmosphere is nitrogen, and the irradiation time is 3-10 minutes; In the mixture of hydroxy silicone oil and methacrylate isocyanate, n(OH):n(NCO)=1~2:1~2; The amount of dibutyltin dilaurate used is 2% to 8% of the mass of methacrylate isocyanate.

3. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The acrylic acid is at least one of acrylic acid and methacrylic acid; The acrylic acid ester monomer is a mixture of one or more of hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, ethylene glycol dimethacrylate, polyethylene glycol 600 dimethacrylate, and polyethylene glycol diacrylate; Preferably: component B is acrylic acid and acrylic acid ester in a mass ratio of 3-8:20-80, or component B is acrylic acid ester and vinyl pyrrolidone in a mass ratio of 20-70:10-15; It is further preferred that: component B is hydroxyethyl methacrylate, methacrylic acid and ethylene glycol dimethacrylate in a mass ratio of 30-80:3-8:3-8; or component B is hydroxyethyl methacrylate, methacrylic acid and polyethylene glycol 600 dimethacrylate in a mass ratio of 30-80:3-8:3-8; or component B is hydroxyethyl methacrylate, vinyl pyrrolidone and polyethylene glycol 600 dimethacrylate in a mass ratio of 20-80:10-20:3-8; Or component B is hydroxyethyl methacrylate, methacrylic acid and polyethylene glycol 600 dimethacrylate in a mass ratio of 10-30:3-8:3-8.

4. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 2, Features: The solvent is a mixture of one or more of dichloromethane, chloroform, tetrachloromethane, isopropanol, methanol, ethanol, butanol and water.

5. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The initiator includes a photoinitiator and a thermal initiator.

6. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 5, Features: The initiator is azobisisoheptanenitrile, azobisisobutyronitrile, benzoyl peroxide, diisopropyl peroxide, ditert-butyl peroxide, diisopropyl peroxydicarbonate, potassium persulfate, ammonium persulfate, hydrogen peroxide, hydroperoxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenylketone, methyl benzoylformate, benzoin dimethyl ether, diphenylacetophenone, α-aminoalkylphenone, dibenzoylphenylphosphine oxide, benzophenone, diphenyl (2,4,6-trimethylbenzoyl)phosphine oxide, 2,2-dimethoxyphenylacetophenone, 2-Hydroxy-4-(2-hydroxyethoxy)-2-methylpropiophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-dimethylaminoethyl benzoate, 2-methylbenzophenone, 4-methylbenzophenone, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether mixture, benzoin isobutyl ether, a blend of benzoin n-butyl ether and benzoin isobutyl ether, α,α-diethoxyacetophenone, α,α-di-(n-butoxy)-acetophenone, isopropylthioxanthone, oxalic acid, alcohol, amine, glucose, sodium bisulfite, sodium thiosulfate, thiol, cyclopentaneate, and one or more of an organic metal compound.

7. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The concentration of the mixed monomers in the modified polyorganosiloxane hybrid silicon mixed monomer solution is 40% to 70%.

8. The modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The weight of the initiator is 0.1-2% of the weight of the mixed monomers.

9. A method for preparing the modified polyorganosiloxane hybrid silicone hydrogel contact lens according to claim 1, Features: The method comprises placing a modified polyorganosiloxane hybrid silicon mixed monomer solution in a mold and preparing the obtained product at -10°C to 100°C through a light-induced polymerization or a heat-induced polymerization process.