Intrinsic high-thermal-conductivity polysiloxane, preparation method thereof and high polymer material
Dehydrobromination by using 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and a basic catalyst in polysiloxane with vinyl-terminated polydimethylsiloxane The silicon-oxygen addition reaction forms intrinsically high thermal conductivity polysiloxane with a layered structure, which solves the problem of low thermal conductivity of polysiloxane and achieves a significant increase in thermal conductivity and maintenance of elastic properties.
Patent Information
- Application Number
- CN202410861484.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-15
AI Technical Summary
The thermal conductivity of existing polysiloxane is low and the orientation effect of liquid crystal small molecules is poor. It is difficult to retain the high molecular chain orientation at room temperature, resulting in thermal conductivity that does not meet expectations.
During the synthesis and processing of polysiloxane, 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and an alkaline catalyst are used for dehydrobromination reaction to obtain small molecule liquid crystal monomers, which are then combined with Vinyl-terminated polydimethylsiloxane and hydrosilylation catalyst Perform silicon-oxygen addition reaction to form intrinsically high thermal conductive polysiloxane with benzene ring, biphenyl group and siloxane chain, utilizing the π- of rigid biphenyl group side chain and flexible polysiloxane main chain The π stacking structure inhibits the random orientation of molecular chains and forms an ordered domain with a layered structure.
The thermal conductivity of polysiloxane is significantly increased by about 70%, maintaining the elastic properties of polysiloxane while having excellent thermal conductivity. The thermal conductivity is increased to 0.34W/(m·K).
Smart Images

Figure CN118772416A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an intrinsic high thermal conductive polysiloxane and a preparation method and a polymer material thereof. Background Art
[0002] The unique organic-inorganic hybrid molecular structure of polysiloxane gives it many properties superior to traditional rubber, such as high and low temperature resistance, low glass transition temperature, weather resistance, wear resistance, electrical insulation, flame retardancy, high chemical stability and physiological inertness. Since its commercialization in the 1940s, polysiloxane has been widely used in various industries such as aerospace, national defense, automobiles, construction, electronics, medical and food processing. For example, it is used as thermal interface materials for electronic devices, elastic bonding, positioning, heat dissipation, insulation and sealing in industries such as automobiles and instruments, and has attracted much attention in the field of thermal conductive materials.
[0003] The thermal conductivity (λ) of ordinary polysiloxane is around 0.2W / (m·K), which cannot meet the requirements of efficient and fast thermal conductivity. Liquid crystal polysiloxane with a special structure is obtained by changing its molecular chain structure during the synthesis and processing of polysiloxane, or by changing the molecular chain arrangement through external force or external field, which can improve its bulk thermal conductivity while maintaining good mechanical and electrical properties. In previous research work, researchers have found that the thermal conductivity of polysiloxane can be effectively improved by adding small molecule liquid crystal primitives during the cross-linking process of polysiloxane. This is because the liquid crystal primitives can form local ordered domains in the cross-linked structure of polysiloxane, which improves the orderliness of the cross-linked structure of polysiloxane, thereby improving the thermal conductivity of polysiloxane. However, the liquid crystal temperature of most liquid crystal small molecules is not uniform with the cross-linking temperature of polysiloxane, making it difficult for polysiloxane to retain the high orientation of the molecular chain in its liquid crystal range at room temperature after cross-linking, and the λ of the prepared intrinsic thermal conductive polysiloxane is far less than the expected design value.
[0004] Therefore, there is an urgent need to research and develop polysiloxane matrix with excellent intrinsic λ. Summary of the invention
[0005] In order to overcome the technical problems in the prior art that polysiloxane has a low intrinsic thermal conductivity and its liquid crystal small molecule orientation effect is poor, the purpose of the present invention is to provide an intrinsic high thermal conductivity polysiloxane and a preparation method and polymer material thereof, wherein the intrinsic high thermal conductivity polysiloxane prepared by the method has excellent intrinsic thermal conductivity.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present application provides an intrinsically highly thermally conductive polysiloxane, the structural formula of which is as follows:
[0008]
[0009] Among them, the value range of n is 0 to 182, the value range of m is 0 to 182, and the value range of p is 23 to 45.
[0010] In combination with the first aspect, preferably, the number average molecular weight of the intrinsic high thermal conductive polysiloxane is 50,000-100,000.
[0011] In combination with the first aspect, preferably, the relationship between n and m is n+m=182.
[0012] The second aspect of the present application provides a method for preparing the intrinsic high thermal conductive polysiloxane according to the first aspect, comprising the following steps:
[0013] Dissolving 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and a basic catalyst in a first organic solvent, and performing a dehydrobromination reaction to obtain a first compound;
[0014] The first compound, vinyl-terminated polydimethylsiloxane, a hydrosilylation catalyst and dimethyl methyl hydrogen are subjected to a siloxane addition reaction to obtain an intrinsic high thermal conductive polysiloxane.
[0015] In combination with the second aspect, preferably, the molar ratio of the 4,4-dihydroxybiphenyl to the 6-bromo-1-hexene is 10:20-23;
[0016] The molar ratio of the 4,4-dihydroxybiphenyl to the alkaline catalyst is 10:20-23.
[0017] In combination with the second aspect, preferably, the alkaline catalyst is one or more of potassium carbonate and potassium iodide;
[0018] The first organic solvent is acetone;
[0019] The hydrosilylation catalyst is one or more of chloroplatinic acid, Karstedt's catalyst and chloroplatinic acid complex.
[0020] In combination with the second aspect, preferably, the molar ratio of the first compound to the vinyl-terminated polydimethylsiloxane is 1:0.5-1.5;
[0021] The molar ratio of the sum of the molar amounts of the first compound and the vinyl-terminated polydimethylsiloxane to the dimethyl methyl hydrogen (siloxane to polysiloxane) is 1.4-1.6:1;
[0022] The molar ratio of the first compound to the hydrosilylation catalyst is 9.5-10.5:0.1.
[0023] In combination with the second aspect, preferably, the temperature for the dehydrobromination reaction is 60° C., and the reaction time is 12-24 h.
[0024] In combination with the second aspect, preferably, the temperature for the silicon-oxygen addition reaction is 110-120° C., and the reaction time is 6-12 hours.
[0025] The third aspect of the present invention provides a polymer material, comprising the intrinsic high thermal conductivity polysiloxane described in the first aspect or the intrinsic high thermal conductivity polysiloxane prepared by the method described in the second aspect.
[0026] Compared with the prior art, the beneficial effects of the present invention include at least:
[0027] The intrinsic high thermal conductivity polysiloxane provided by the present invention contains a benzene ring, a biphenyl group (rigid mesogen) and a silicon-oxygen-silicon chain (flexible chain) in its structural unit, and the molecular chain is locally ordered. The flexible polysiloxane main chain has a large free volume and molecular weight; the stacking of the rigid biphenyl group side chains and the π-π stacking structure between molecules inhibit the random orientation of the molecular chain and promote the formation of ordered domains of the layered structure. The flexible polysiloxane main chain and the rigid biphenyl group side chains cooperate with each other, so that the intrinsic high thermal conductivity polysiloxane has excellent thermal conductivity while maintaining the elastic properties of the polysiloxane. The thermal conductivity of the intrinsic high thermal conductivity polysiloxane provided by the present application is 0.34W / (m·K), which is about 70% higher than the thermal conductivity of the general polysiloxane (0.20W / (m·K)).
[0028] The preparation method of the intrinsic high thermal conductivity polysiloxane provided by the present invention first uses 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and an alkaline catalyst as main raw materials, and synthesizes a small molecule liquid crystal monomer through a dehydrobromination reaction; the dehydrobromination reaction product is subjected to a hydrosilylation reaction with a vinyl-terminated polydimethylsiloxane, a hydrosilylation catalyst and dimethylmethyl hydrogen (siloxane and polysiloxane) to prepare an intrinsic high thermal conductivity polysiloxane. On the one hand, the stacking of the rigid biphenyl group side chains and the π-π stacking structure between molecules inhibit the random orientation of the molecular chain, thereby promoting the formation of ordered domains of the layered structure. On the other hand, the flexible polysiloxane main chain and the rigid biphenyl element side chains cooperate with each other, so that the intrinsic high thermal conductivity polysiloxane has excellent thermal conductivity while maintaining the elastic properties of the polysiloxane. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A hydrogen nuclear magnetic resonance spectrum of the first compound provided in an embodiment of the present invention;
[0030] Figure 2 Fourier transform infrared spectra of the mixture 1 and the intrinsic high thermal conductive polysiloxane prepared in Examples 1-4;
[0031] Figure 3Polarized light microscope photographs of the intrinsic high thermal conductive polysiloxane prepared in Example 1, wherein (a) is at room temperature, (b) is at the crystal melting temperature, and (c) is above the crystal melting temperature. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0033] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present invention have the same meaning as those commonly understood by those skilled in the art to which the embodiments of the present invention pertain. The terms used in the embodiments of the present invention are only for the purpose of describing the embodiments of the present invention and are not intended to limit the present invention.
[0034] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0035] It should be noted that all raw materials / reagents in the embodiments of the present invention can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the embodiments of the present invention is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, wherein A and B can be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0036] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0037] Those skilled in the art should understand that in the following description of the embodiments of the present invention, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.
[0038] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "an" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0039] It will be appreciated by those skilled in the art that the numerical ranges in the embodiments of the present invention are to be understood as also specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0040] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present invention. All documents mentioned in this specification are generally incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present invention shall prevail.
[0041] It should be noted that all raw materials and / or reagents in the examples of the present invention are purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0042] In a first aspect, an embodiment of the present invention provides an intrinsically highly thermally conductive polysiloxane, the structural formula of the intrinsically highly thermally conductive polysiloxane is as follows:
[0043]
[0044] In a specific embodiment, the number average molecular weight of the intrinsic thermal conductive liquid polysiloxane in the embodiment of the present invention is preferably 50,000-100,000, more preferably 75,000-100,000, and further preferably 90,000-100,000.
[0045] The intrinsic high thermal conductivity polysiloxane provided in the embodiment of the present invention includes a flexible polysiloxane main chain and a rigid biphenyl group side chain in its structural unit, specifically containing a benzene ring, a biphenyl group (rigid mesogen) and a silicon-oxygen-silicon chain (flexible chain), and the molecular chain is locally ordered. The flexible polysiloxane main chain has a large free volume and molecular weight; the stacking of the rigid biphenyl group side chains and the π-π stacking structure between molecules inhibit the random orientation of the molecular chain and promote the formation of ordered domains of the layered structure. The flexible polysiloxane main chain and the rigid biphenyl group side chain cooperate with each other, so that the intrinsic high thermal conductivity polysiloxane has excellent thermal conductivity while maintaining the elastic properties of the polysiloxane. The thermal conductivity of the intrinsic high thermal conductivity polysiloxane provided by the present invention is 0.34W / (m·K), which is about 70% higher than the general thermal conductivity of polysiloxane (0.20W / (m·K)).
[0046] In a second aspect, an embodiment of the present invention provides a method for preparing an intrinsically highly thermally conductive polysiloxane, the method comprising the following steps S10 to S20:
[0047] S10: dissolving 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and a basic catalyst in a first organic solvent, and performing a dehydrobromination reaction to obtain a first compound;
[0048] S20: mixing the first compound, vinyl-terminated polydimethylsiloxane, a silylation catalyst and dimethyl methyl hydrogen (siloxane and polysiloxane) to perform a silylation reaction to obtain an intrinsic high thermal conductivity polysiloxane.
[0049] It should be noted that the number average molecular weight of the intrinsic high thermal conductive polysiloxane in the embodiment of the present invention is preferably 100,000.
[0050] It should be noted that in the above step S10, 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and an alkaline catalyst are dissolved in a first organic solvent to carry out a dehydrobromination reaction, preferably the following steps: 4,4-dihydroxybiphenyl and the first organic solvent are mixed to obtain a 4,4-dihydroxybiphenyl solution; 6-bromo-1-hexene, potassium carbonate and potassium iodide are added to the 4,4-dihydroxybiphenyl solution in sequence.
[0051] It should be noted that, when 4,4-dihydroxybiphenyl and the first organic solvent are mixed, it is preferably carried out under magnetic stirring conditions; in the present invention, there is no particular limitation on the stirring rate and time, as long as the components can be mixed uniformly.
[0052] It should be noted that the preferred method of adding 6-bromo-1-hexene in the present invention is dropwise addition; and the present invention has no particular limitation on the dropwise addition rate and time, and the dropwise addition rate and time known to those skilled in the art can be used.
[0053] It should be noted that the above dehydrobromination reaction is carried out under water bath conditions; after the above dehydrobromination reaction is completed, the present invention preferably performs rotary evaporation, first drying, first washing, second washing and second drying on the reaction product in sequence to obtain the first compound.
[0054] It should be noted that in the present invention, the temperature of the first drying is preferably 65-85° C., and the drying time is preferably 12-24 hours. In the present invention, the first drying method is preferably vacuum drying; and the vacuum drying is preferably performed in a vacuum drying oven.
[0055] It should be noted that the washing liquid used in the first washing is preferably distilled water; the washing liquid used in the second washing is preferably anhydrous ethanol; the washing method is preferably stirring in the washing liquid for 24 hours and then filtering, and the number of washing times for each washing liquid is preferably 2-4 times.
[0056] It should be noted that after washing, the present invention preferably dries the washed material.
[0057] It should be noted that the present invention does not impose any specific limitation on the parameters of the rotary evaporation, as long as the first organic solvent can be removed.
[0058] It should be noted that in the present invention, the temperature of the second drying is preferably 55-65° C., and the drying time is preferably 12-24 hours. In the present invention, the second drying method is preferably vacuum drying; and the vacuum drying is preferably performed in a vacuum drying oven.
[0059] In a specific embodiment, the hydrosilylation catalyst in the embodiment of the present invention is preferably one or more of chloroplatinic acid, Karstedt's catalyst and chloroplatinic acid complex, wherein the chloroplatinic acid complex is various complexes of chloroplatinic acid having the function of catalyzing the hydrosilylation reaction.
[0060] It should be noted that the mixing of the first compound, vinyl-terminated polydimethylsiloxane, hydrosilylation catalyst and dimethylmethyl hydride (siloxane and polysiloxane) in the above step S20 preferably includes the following steps: mixing the first compound with vinyl-terminated polydimethylsiloxane to obtain a mixture; adding the hydrosilylation catalyst to the above mixture, stirring evenly and then adding dimethylmethyl hydride (siloxane and polysiloxane). The mixture is evacuated to remove bubbles and poured into a mold. In the present invention, the mixing of the first compound, vinyl-terminated polydimethylsiloxane, Karstedt's catalyst and dimethylmethyl hydride (siloxane and polysiloxane) is preferably carried out under magnetic stirring.
[0061] In a specific embodiment, when the silicon-oxygen addition reaction is carried out in the embodiment of the present invention, the reaction temperature is preferably 110-120° C., and the reaction time is preferably 6-12 hours.
[0062] It should be noted that after the hydrosilylation reaction, the present invention preferably sequentially performs a first adsorption, a first filtration, a rotary evaporation, a first drying, a second extraction, a second rotary evaporation and a second drying on the obtained hydrosilylation reaction liquid to obtain the first compound.
[0063] The preparation method of the intrinsic high thermal conductivity polysiloxane provided by the embodiment of the present invention is firstly to synthesize a small molecule liquid crystal monomer by dehydrobromination reaction with 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and alkaline catalyst as main raw materials; the dehydrobromination reaction product is subjected to hydrosilylation reaction with vinyl-terminated polydimethylsiloxane, hydrosilylation catalyst and dimethylmethyl hydrogen (siloxane and polysiloxane) to prepare an intrinsic high thermal conductivity polysiloxane. On the one hand, the stacking of rigid biphenyl group side chains and the π-π stacking structure between molecules inhibit the random orientation of the molecular chain, thereby promoting the formation of ordered domains of the layered structure. On the other hand, the flexible polysiloxane main chain cooperates with the rigid biphenyl element side chain, so that the intrinsic high thermal conductivity polysiloxane has excellent thermal conductivity while maintaining the elastic properties of polysiloxane.
[0064] In a specific embodiment, the molar ratio of 4,4-dihydroxybiphenyl and the 6-bromo-1-hexene in the embodiment of the present invention is 10:20-23; more preferably 10:21. Wherein, when the molar ratio of 4,4-dihydroxybiphenyl and 6-bromo-1-hexene is less than 10:23, due to the excess of 6-bromo-1-hexene, the dehydrobromination reaction is incomplete, so that a large amount of 6-bromo-1-hexene remains in the product; when the molar ratio of 4,4-dihydroxybiphenyl and 6-bromo-1-hexene is greater than 10:20, 4,4-dihydroxybiphenyl is excessive, and a large amount of 4,4-dihydroxybiphenyl remains in the product; when the molar ratio of 4,4-dihydroxybiphenyl and 6-bromo-1-hexene is preferably 10:21, the dehydrobromination reaction is completely carried out, and a small amount of 6-bromo-1-hexene remains, which can be completely removed by subsequent washing.
[0065] In a specific embodiment, the molar ratio of 4,4-dihydroxybiphenyl to the alkaline catalyst in the embodiment of the present invention is preferably 10:20-23. When the molar ratio of 4,4-dihydroxybiphenyl to the alkaline catalyst is less than 10:23, the alkaline catalyst is excessive and the alkaline catalyst remains in the product; when the molar ratio of 4,4-dihydroxybiphenyl to the alkaline catalyst is greater than 10:20, the 4,4-dihydroxybiphenyl is excessive, the alkaline catalyst cannot completely react with the hydroxyl group in the 4,4-dihydroxybiphenyl, the dehydrobromination reaction is incomplete, and the 4,4-dihydroxybiphenyl remains in the product.
[0066] In a specific embodiment, the alkaline catalyst in the embodiment of the present invention is preferably one or more of potassium carbonate, potassium iodide and potassium hydroxide; more preferably a mixture of potassium carbonate and potassium iodide.
[0067] The reaction mechanism of the alkaline catalyst is that the hydroxide ions in the alkaline catalyst act as nucleophiles to attack the halogen atoms in the organic halogen compound, causing it to release halogen atoms to generate a dehydrobromination reaction of an aromatic compound. The alkaline catalyst can promote the removal of halogen atoms from the halogen compound, causing p-hydroxybiphenyl to lose one molecule of alcohol to obtain one molecule of the first compound and hydrogen bromide.
[0068] It should be noted that when the alkaline catalyst is a mixture of potassium carbonate and potassium iodide, the molar ratio of potassium carbonate to potassium iodide is 6:1.
[0069] In a specific embodiment, the temperature for the dehydrobromination reaction in the embodiment of the present invention is preferably 40-65°C, more preferably 60-65°C; the reaction time is preferably 24-48h, more preferably 36-48h, and most preferably 40-48h.
[0070] In a specific embodiment, the first organic solvent in the embodiment of the present invention is preferably acetone, which has the advantage of having good solubility for the reactants and can promote the forward progress of the reaction.
[0071] In a specific embodiment, the hydrosilylation catalyst in the embodiment of the present invention includes one or more of chloroplatinic acid, Karstedt's catalyst and chloroplatinic acid complex.
[0072] The hydrosilylation catalyst can promote the addition reaction between the carbon-carbon double bond on the first compound and the active hydrogen on dimethylmethyl hydrogen (siloxane and polysiloxane) to generate new silicon-carbon bonds.
[0073] In a specific embodiment, the molar ratio of the sum of the first compound and the vinyl-terminated polydimethylsiloxane in the embodiment of the present invention to dimethylmethyl hydrogen (siloxane and polysiloxane) is preferably 1.4-1.6:1; more preferably 1.5:1. Among them, when the molar ratio of the sum of the first compound and the vinyl-terminated polydimethylsiloxane to dimethylmethyl hydrogen (siloxane and polysiloxane) is less than 1.4:1, the reaction is incomplete, and a large amount of active hydrogen remains in the polysiloxane, which will undergo a cross-linking reaction with water and oxygen in the air, reducing the flexibility of the polysiloxane; when the molar ratio of the sum of the first compound and the vinyl-terminated polydimethylsiloxane to dimethylmethyl hydrogen (siloxane and polysiloxane) is greater than 1.6:1, the first compound remains in the product, so that the liquid crystal small molecules do not have a good destination effect, affecting the thermal conductivity.
[0074] The amount of the first compound cannot be 0, and the amount of the vinyl-terminated polydimethylsiloxane can be 0.
[0075] It should be noted that, when the hydrosilylation catalyst is preferably Karstedt's catalyst, the molar ratio of the first compound to the Karstedt's catalyst is preferably 9.5-10.5:0.1, more preferably 10:0.1.
[0076] The technical method of the present invention will be further described below in conjunction with specific embodiments.
[0077] Example 1
[0078] This embodiment provides a method for preparing an intrinsically highly thermally conductive polysiloxane, and the specific steps are as follows:
[0079] (1) Dissolving 4,4-dihydroxybiphenyl, 6-bromo-1-hexene, potassium carbonate and potassium iodide in a first organic solvent and performing a dehydrobromination reaction to obtain a first compound:
[0080] The specific process is as follows: 3.724g (20mmol) 4,4-dihydroxybiphenyl, 5.796g (42mmol) potassium carbonate and 0.6g (7mmol) potassium iodide are dissolved in 70mL acetone, stirred until clear and transparent, and then 6.846g (42mmol) 6-bromo-1-hexene is slowly dripped thereinto, and the resulting mixture is condensed and refluxed at 60°C for 48h. Afterwards, the reaction mixture is cooled to room temperature, the excess solvent is removed by rotary evaporation, the product is washed with a large amount of deionized water, and then washed twice with ethanol. The filtrate is removed, the filter cake is collected, and the first compound is obtained after vacuum drying for 8h.
[0081] (2) The first compound, vinyl-terminated polydimethylsiloxane, a hydrosilylation catalyst and dimethylmethyl hydrogen (siloxane and polysiloxane) are subjected to a siloxane addition reaction to obtain an intrinsically highly thermally conductive polysiloxane:
[0082] The specific process is as follows: 0.175g (0.5mmol) of the first compound and 7.404g (1mmol) of vinyl-terminated polydimethylsiloxane are mixed and stirred evenly, 4μL of Karstedt's catalyst is added to the above mixture, and 8g (1mmol) of dimethyl methyl hydride (siloxane and polysiloxane) is added. The mixture is vacuumed to remove bubbles, poured into a mold, and reacted at 110°C for 8h to obtain intrinsic high thermal conductivity polysiloxane PDMS. Ⅱ , its intrinsic thermal conductivity is 0.28W / (m·K).
[0083] Example 2
[0084] This embodiment 2 provides a method for preparing an intrinsically highly thermally conductive polysiloxane, and the specific steps are as follows:
[0085] Intrinsic high thermal conductivity polysiloxane was prepared according to the method of Example 1, except that in step (2), 0.35 g (1 mmol) of the first compound and 3.702 g (0.5 mmol) of vinyl-terminated polydimethylsiloxane were mixed and stirred evenly, 4 μL of Karstedt's catalyst was added to the above mixture, and 8 g (1 mmol) of dimethyl methyl hydride (siloxane and polysiloxane) was added. The mixture was evacuated to remove bubbles, poured into a mold, and reacted at 110° C. for 8 h to obtain intrinsic high thermal conductivity polysiloxane PDMS. Ⅲ .
[0086] It should be noted that the intrinsic high thermal conductivity polysiloxane PDMS Ⅲ The intrinsic thermal conductivity is 0.34W / (m·K).
[0087] Example 3
[0088] This embodiment 3 provides a method for preparing an intrinsically highly thermally conductive polysiloxane, and the specific steps are as follows:
[0089] Intrinsic high thermal conductivity polysiloxane was prepared according to the method of Example 1, except that in step (2), 0.623 g (1.5 mmol) of the first compound and 0 g (0 mmol) of vinyl-terminated polydimethylsiloxane were mixed and stirred uniformly, 4 μL of Karstedt's catalyst was added to the above mixture, and 8 g (1 mmol) of dimethyl methyl hydride (siloxane and polysiloxane) was added. The mixture was evacuated to remove bubbles, poured into a mold, and reacted at 110° C. for 8 h to obtain intrinsic high thermal conductivity polysiloxane PDMS. Ⅲ .
[0090] It should be noted that the intrinsic high thermal conductivity polysiloxane PDMS Ⅳ The intrinsic thermal conductivity is 0.30W / (m·K).
[0091] Example 4
[0092] This embodiment provides a method for preparing an intrinsically highly thermally conductive polysiloxane, and the specific steps are as follows:
[0093] (1) 20 mmol of 4,4-dihydroxybiphenyl was added to 70 mL of acetone, and magnetic stirring was performed to mix the mixture evenly. Then, 40 mmol of a mixture of potassium carbonate and potassium iodide (the molar ratio of potassium carbonate to potassium iodide was 6:1) was added in sequence, and stirred until it became clear and transparent. Subsequently, 40 mmol of 6-bromo-1-hexene was slowly added dropwise thereto, and the resulting mixture was condensed and refluxed at 40° C. for 48 h. Thereafter, the reaction mixture was cooled to room temperature, the excess solvent was removed by rotary evaporation, dried at 65° C. for 24 h, stirred in a large amount of distilled water for 24 h, washed twice, stirred in anhydrous ethanol for 24 h, washed twice, the filtrate was removed, the filter cake was collected, and vacuum dried at 65° C. for 8 h to obtain the first compound.
[0094] (2) 0.5 mmol of the first compound and 1 mmol of vinyl-terminated polydimethylsiloxane are mixed and stirred to obtain a mixture, 0.005 mmol of Karstedt's catalyst is added to the mixture, and after stirring, 1 mmol of dimethyl methyl hydrogen (siloxane and polysiloxane) is added, and then vacuuming is performed to remove bubbles, and the mixture is poured into a mold, and reacted at 120° C. for 6 hours to obtain intrinsic high thermal conductivity polysiloxane.
[0095] Example 5
[0096] (1) 20 mmol of 4,4-dihydroxybiphenyl was added to 70 mL of acetone, and magnetic stirring was performed to mix the mixture evenly. Then, 46 mmol of a mixture of potassium carbonate and potassium iodide (the molar ratio of potassium carbonate to potassium iodide was 6:1) was added in sequence, and stirred until it became clear and transparent. Subsequently, 44 mmol of 6-bromo-1-hexene was slowly added dropwise thereto, and the resulting mixture was condensed and refluxed at 65° C. for 24 h. Thereafter, the reaction mixture was cooled to room temperature, the excess solvent was removed by rotary evaporation, dried at 65° C. for 24 h, stirred in a large amount of distilled water for 24 h, washed the product three times, stirred in anhydrous ethanol for 24 h, washed twice, the filtrate was removed, the filter cake was collected, and vacuum dried at 55° C. for 8 h to obtain the first compound.
[0097] (2) 0.5 mmol of the first compound and 1 mmol of vinyl-terminated polydimethylsiloxane were mixed and stirred to obtain a mixture, Karstedt's catalyst was added to the mixture, stirred to obtain a mixture, and then 1 mmol of dimethyl methyl hydride (siloxane and polysiloxane) was added, and then vacuumed to remove bubbles, poured into a mold, and reacted at 110° C. for 12 hours to obtain intrinsic high thermal conductivity polysiloxane. The molar ratio of the first compound to the Karstedt's catalyst was 10.5:0.1.
[0098] Example 6
[0099] (1) 20 mmol of 4,4-dihydroxybiphenyl was added to 70 mL of acetone, and magnetic stirring was performed to mix the mixture evenly. Then, 44 mmol of a mixture of potassium carbonate and potassium iodide (the molar ratio of potassium carbonate to potassium iodide was 6:1) was added in sequence, and stirred until it became clear and transparent. Subsequently, 46 mmol of 6-bromo-1-hexene was slowly added thereto, and the resulting mixture was condensed and refluxed at 50° C. for 40 h. Thereafter, the reaction mixture was cooled to room temperature, the excess solvent was removed by rotary evaporation, dried at 85° C. for 12 h, stirred in a large amount of distilled water for 24 h, washed the product four times, stirred in anhydrous ethanol for 24 h, washed three times, the filtrate was removed, the filter cake was collected, and vacuum dried at 60° C. for 8 h to obtain the first compound.
[0100] (2) 0.6 mmol of the first compound and 1 mmol of vinyl-terminated polydimethylsiloxane are mixed and stirred to obtain a mixture, chloroplatinic acid complex and Karstedt's catalyst are added to the mixture, stirred to obtain a mixture, 1 mmol of dimethyl methyl hydride (siloxane and polysiloxane) is added, and then vacuuming is performed to remove bubbles, and the mixture is poured into a mold, and reacted at 115° C. for 10 hours to obtain intrinsic high thermal conductivity polysiloxane. The molar ratio of the first compound to the total molar amount of the chloroplatinic acid complex and the Karstedt's catalyst is 9.5:0.1, and the molar ratio of the chloroplatinic acid complex to the Karstedt's catalyst is 1:1.
[0101] Example 7
[0102] (1) 20 mmol of 4,4-dihydroxybiphenyl was added to 70 mL of acetone, and magnetic stirring was performed to mix the mixture evenly. Then, 42 mmol (the molar ratio of potassium carbonate to potassium iodide was 6:1) was added successively, and stirred until the mixture was clear and transparent. Subsequently, 45 mmol of 6-bromo-1-hexene was slowly dropped thereinto, and the resulting mixture was condensed and refluxed at 55° C. for 36 h. Thereafter, the reaction mixture was cooled to room temperature, the excess solvent was removed by rotary evaporation, dried at 75° C. for 15 h, stirred in a large amount of distilled water for 24 h, washed twice, stirred in anhydrous ethanol for 24 h, washed four times, the filtrate was removed, the filter cake was collected, and vacuum dried at 55° C. for 8 h to obtain the first compound.
[0103] (2) 0.4 mmol of the first compound and 1 mmol of vinyl-terminated polydimethylsiloxane are mixed and stirred to obtain a mixture, 0.004 mmol of chloroplatinic acid catalyst is added to the above mixture, and after stirring, 1 mmol of dimethyl methyl hydrogen (siloxane and polysiloxane) is added, and then vacuum is evacuated to remove bubbles, and the mixture is poured into a mold and reacted at 117° C. for 7 hours to obtain intrinsic high thermal conductivity polysiloxane.
[0104] In order to verify the performance of the intrinsic high thermal conductivity polysiloxane prepared in Examples 1-4 of the present invention, the first compound provided in the present invention was analyzed by hydrogen nuclear magnetic resonance spectrum and Fourier transform infrared spectrum. The results are as follows: Figure 1-Figure 2 shown.
[0105] from Figure 1 It can be seen that the peaks at 6.8ppm and 7.4ppm are characteristic peaks of protons on the biphenyl structure, the multiple peaks at 4.9ppm and 5.7ppm are characteristic peaks of protons on unsaturated carbon-carbon double bonds, and the peaks at 1.4ppm, 1.7ppm, 2.1ppm and 4.0ppm are characteristic peaks of protons on carbon-carbon chains. This proves that there are biphenyl units connected by flexible carbon-carbon chains in the molecular structure.
[0106] from Figure 2 It can be seen that 1017cm -1 and 1065cm -1 The characteristic absorption peak of Si-O-Si is 3037 cm -1 and 3062cm -1 The characteristic absorption peak of the unsaturated carbon-carbon bond at 200 μm disappeared after cross-linking, which proved that the molecular structure of the intrinsic high thermal conductive polysiloxane was consistent with the design.
[0107] In order to verify the liquid crystal properties of the small molecule liquid crystal monomers prepared in Examples 1-4 of the present invention, the intrinsic high thermal conductivity polysiloxanes 1-4 prepared in Examples 1-4 were characterized by polarizing microscope. The results are as follows: Figure 3 shown.
[0108] from Figure 3 It can be seen that the observation area appears bright yellow at room temperature ( Figure 3 In (a), the boundaries between the small molecule liquid crystal monomer particles are clear, indicating that there is microscopic anisotropy in its structure, indicating that the small molecule liquid crystal monomer is a semi-crystalline compound. When the temperature rises to the crystal melting temperature (T lc , the temperature at which the crystal phase transforms into the liquid crystal phase), the small molecule liquid crystal monomer exhibits fluidity, and the field of view of the observation area gradually becomes brighter and more uniform ( Figure 3 (b) indicates that the small molecule liquid crystal monomer has changed from the crystalline state to the liquid crystal state. As the temperature rises further, the bright yellow and green spots (typical nematic phase morphology) disappear, and the field of view is completely transparent ( Figure 3 (c) indicates that the temperature reaches the clearing point (T i , the temperature at which the liquid crystal phase changes to the isotropic phase), the small molecule liquid crystal monomer presents an isotropic liquid state. Therefore, the crosslinking temperature of the intrinsic high thermal conductive polysiloxane is determined to be 120°C.
[0109] The thermal conductivity coefficients of the intrinsic high thermal conductivity polysiloxane materials I-IV of the present invention were tested using a Hot Disk TPS2200 thermal conductivity tester. Ⅰ The intrinsic λ is 0.22W / (m·K), PDMS Ⅱ The intrinsic λ of PDMS is 0.28W / (m·K). Ⅲ The λ reaches 0.34W / (m·K), PDMS Ⅳ The λ reaches 0.30W / (m·K).
[0110] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. An intrinsically highly thermally conductive polysiloxane, characterized in that: The structural formula of the intrinsic high thermal conductivity polysiloxane is as follows: Among them, the value range of n is 0 to 182, the value range of m is 0 to 182, and the value range of p is 23 to 45.
2. The intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The number average molecular weight of the intrinsic high thermal conductive polysiloxane is 50,000-100,000.
3. The intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The relationship between n and m is n+m=182.
4. A method for preparing an intrinsically highly thermally conductive polysiloxane, characterized in that: The following steps are involved: Dissolving 4,4-dihydroxybiphenyl, 6-bromo-1-hexene and a basic catalyst in a first organic solvent, and performing a dehydrobromination reaction to obtain a first compound; The first compound, vinyl-terminated polydimethylsiloxane, a hydrosilylation catalyst and dimethylmethylhydrogen (siloxane and polysiloxane) are subjected to a siloxane addition reaction to obtain an intrinsic high thermal conductive polysiloxane.
5. The method for preparing the intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The molar ratio of the 4,4-dihydroxybiphenyl to the 6-bromo-1-hexene is 10:20-23; The molar ratio of the 4,4-dihydroxybiphenyl to the alkaline catalyst is 10:20-23.
6. The method for preparing the intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The alkaline catalyst is one or more of potassium carbonate and potassium iodide; The first organic solvent is acetone; The hydrosilylation catalyst is one or more of chloroplatinic acid, Karstedt's catalyst and chloroplatinic acid complex.
7. The method for preparing the intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The molar ratio of the first compound to the vinyl-terminated polydimethylsiloxane is 1:0.5-1.5; The molar ratio of the sum of the molar amounts of the first compound and the vinyl-terminated polydimethylsiloxane to the dimethyl methyl hydrogen (siloxane to polysiloxane) is 1.4-1.6:1; The molar ratio of the first compound to the hydrosilylation catalyst is 9.5-10.5:0.
1.
8. The method for preparing the intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The temperature for the dehydrobromination reaction is 60° C., and the reaction time is 12-24 hours.
9. The method for preparing the intrinsically highly thermally conductive polysiloxane according to claim 1, characterized in that: The temperature for the silicon-oxygen addition reaction is 110-120° C., and the reaction time is 6-12 hours.
10. A polymer material, characterized in that: The invention comprises the intrinsic high thermal conductivity polysiloxane according to any one of claims 1 to 3 or the intrinsic high thermal conductivity polysiloxane prepared by the method according to any one of claims 4 to 9.
Citation Information
Cited By
Flexible intrinsic heat-conducting polysiloxane composite material and preparation method thereof