Oily paint for stainless steel and aluminum breaking material, preparation method and application
By using oil-based coatings that combine epoxy resin and nanomaterials on stainless steel and broken aluminum materials, the problems of insufficient adhesion, corrosion resistance and environmental performance of existing coatings are solved, achieving high-performance coating formation and environmental friendliness. coating preparation for high-end applications.
Patent Information
- Application Number
- CN202410975173.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing coatings have insufficient surface adhesion, corrosion resistance, and environmental performance on stainless steel and broken aluminum materials, cannot meet the needs of high-end applications, and contain a large amount of volatile organic compounds that are harmful to the environment and human health.
Epoxy resin is used as the base resin, combined with nano-silica, nano-titanium dioxide, lignin nano-microspheres and halloysite nanotubes-aluminum tripolyphosphate composite to form a wear-resistant and corrosion-resistant oily coating. Through a specific preparation method Improve the hardness, protective performance and environmental friendliness of the coating.
The prepared coating has excellent wear resistance and corrosion resistance, good adhesion, and significantly improved environmental performance. It is suitable for industrial production and can effectively protect stainless steel and broken aluminum materials.
Smart Images

Figure BDA0004954317400000071 
Figure BDA0004954317400000081 
Figure BDA0004954317400000082
Abstract
Description
Technical Field
[0001] The present application relates to the field of coating technology, and in particular to an oily coating for stainless steel and aluminum materials, a preparation method and application thereof. Background Art
[0002] At present, there are many kinds of oily coatings on the market, but there are relatively few special coatings for stainless steel and broken aluminum materials. Existing coatings have deficiencies in adhesion, corrosion resistance, wear resistance, etc., and cannot meet the needs of high-end applications. Traditional oily coatings usually use organic solvents as diluents and contain a large amount of volatile organic compounds (VOCs), which are harmful to the environment and human health. At the same time, the formula and process of existing coatings make it difficult to form strong adhesion and excellent corrosion resistance on the surface of stainless steel and broken aluminum materials. Existing oily coatings have deficiencies in environmental performance, adhesion and corrosion resistance, and cannot meet the high-end application needs of stainless steel and broken aluminum materials. Summary of the invention
[0003] In order to solve at least one of the above technical problems, an oily coating for stainless steel and broken aluminum materials with strong adhesion, excellent wear resistance and corrosion resistance and environmental protection is developed. The present application provides an oily coating for stainless steel and broken aluminum materials, a preparation method and application.
[0004] On the one hand, the present application provides an oily coating for stainless steel and broken aluminum materials, comprising the following components in parts by weight: 60-80 parts of epoxy resin, 8-15 parts of curing agent, 30-50 parts of organic solvent, 10-15 parts of nano-silicon dioxide, 5-10 parts of nano-titanium dioxide, 8-14 parts of halloysite nanotube-aluminum tripolyphosphate complex, 12-21 parts of lignin nano-microspheres, 2-4 parts of dispersant, 1-3 parts of defoaming agent, and 2-4 parts of leveling agent.
[0005] Through the above technical solution, this application selects epoxy resin as the base resin of the coating, which has good adhesion and corrosion resistance; Nano-silica as a filler pigment can enhance the hardness and wear resistance of the coating, while improving the scratch resistance. Nano-sized silica can also improve the rheology and thixotropy of the coating. Nano-titanium dioxide can provide hiding power and UV protection, while enhancing the weather resistance and anti-chalking ability of the coating. Titanium dioxide is also a common white pigment; Lignin nanoparticles are derived from lignin in plant biomass and are renewable biomass resources. The use of lignin nanoparticles can improve the environmental friendliness of the coating. After nano-processing, they can be used as a reinforcing agent to increase the overall hardness and density of the coating, thereby enhancing its ability to resist wear and tear, and may provide additional environmental protection properties. Halloysite nanotube-aluminum tripolyphosphate composite can significantly improve the corrosion resistance of the coating. Halloysite nanotubes have a hollow tubular structure, which can act as a physical barrier to prevent corrosive media such as oxygen, moisture and electrolytes from penetrating into the surface of the substrate, thereby delaying the corrosion process; aluminum tripolyphosphate, as a corrosion inhibitor, can decompose under corrosive conditions to produce phosphate ions, which can react with metal ions on the surface of the metal substrate to form a dense protective film to further block the corrosive media.
[0006] Optionally, the method for preparing the lignin nanospheres comprises the following steps: A1. Mix enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water, and disperse by ultrasonication for 20-30 min to completely dissolve the lignin. Then, centrifuge at 7000-8000 rpm for 20-25 min, and take the supernatant to obtain a lignin solution. A2, injecting the prepared lignin solution into ultrapure water to prepare a lignin micro-nanosphere suspension; A3. Add the lignin micro-nanosphere suspension into an autoclave, heat it at 160-180° C. for 10-12 hours, and then freeze-dry it to obtain the lignin nano-microspheres.
[0007] Optionally, in step A1, the weight ratio of the enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water is (20-25):(8-10):1; in step A2, the volume ratio of the lignin solution to ultrapure water is 1:(3-5).
[0008] Optionally, the preparation method of the halloysite nanotube-aluminum tripolyphosphate composite comprises the following steps: B1, adding a hydrochloric acid solution with a concentration of (3-5) mol / L to the halloysite nanotubes, heating and stirring in a water bath for 4-6 hours, centrifuging, filtering, washing, and grinding to obtain the halloysite nanotubes after hydrochloric acid etching; B2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step B1, aluminum tripolyphosphate and deionized water, ultrasonically dispersing for 40-60 minutes, and then vacuum drying the obtained suspension; B3. After vacuum drying, centrifugation is performed to separate the solid phase, and the solid phase is washed, dried, and ground into powder to obtain the halloysite nanotube-corrosion inhibitor composite.
[0009] Optionally, the weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step B1 is (5-7):(60-80); the weight ratio of the aluminum tripolyphosphate and deionized water in step B2 to the halloysite nanotubes in step B1 is (6-8):(50-60):1.
[0010] Optionally, the weight ratio of the halloysite nanotube-aluminum tripolyphosphate composite to the lignin nanospheres is 1:(1-1.8).
[0011] Through the above technical solution, the present application defines the weight ratio between the lignin nano-microspheres and the halloysite nanotube-aluminum tripolyphosphate composite, ensuring that the coating has excellent wear resistance and corrosion resistance.
[0012] Optionally, the curing agent is a modified amine curing agent; the organic solvent is butyl acetate; the dispersant is sodium dodecyl sulfate; the defoaming agent is BYK024; and the leveling agent is an organic silicone leveling agent.
[0013] In a second aspect, the present application provides a method for preparing the oily coating for the above-mentioned stainless steel and aluminum materials, comprising the following steps: S1, mixing the epoxy resin, organic solvent, defoamer and dispersant uniformly; S2, adding the nano-silicon dioxide, nano-titanium dioxide, lignin nano-microspheres and halloysite nanotube-aluminum tripolyphosphate complex, and stirring at a rotation speed of 700-800 rpm for 1-1.5 hours; S3, adding the leveling agent and curing agent, stirring for 4-8 minutes at a rotation speed of 500-600rpm, to obtain the oily coating for the stainless steel and aluminum materials.
[0014] Through the above technical scheme, the oily coating for stainless steel and aluminum materials prepared in the present application has excellent wear resistance and corrosion resistance, a simple preparation method, and is suitable for industrial production.
[0015] On the third aspect, the present application provides the application of the above-mentioned oily coating for stainless steel and broken aluminum materials in the field of preparing wear-resistant and anti-corrosion coatings. The oily coating for stainless steel and broken aluminum materials is coated on a pretreated substrate and dried to obtain an anti-corrosion and wear-resistant coating.
[0016] Through the above technical scheme, the coating prepared in the present application can be coated on stainless steel and broken aluminum materials to form a coating with excellent wear resistance and corrosion resistance, good adhesion, and can better provide protection for stainless steel and broken aluminum materials.
[0017] Optionally, the substrate is one of stainless steel and aluminum alloy; the pretreatment includes degreasing, rust removal and grinding; the drying temperature is 60-80°C and the drying time is 1-1.5h.
[0018] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application uses epoxy resin as the base resin of the coating, which has good adhesion and corrosion resistance; nano-silicon dioxide is used as a filler pigment to enhance the hardness and wear resistance of the coating, while improving the scratch resistance. Nano-sized silicon dioxide can also improve the rheology and thixotropy of the coating; nano-titanium dioxide can provide hiding power and UV protection, while enhancing the weather resistance and anti-powdering ability of the coating. Titanium dioxide is also a common white pigment; lignin nano-microspheres are derived from lignin in plant biomass, which is a renewable biomass resource. The use of lignin nano-microspheres can improve the environmental friendliness of the coating. After nano-treatment After treatment, it can act as a reinforcing agent to increase the overall hardness and density of the coating, thereby enhancing its ability to resist wear and possibly providing additional environmentally friendly properties; the halloysite nanotube-aluminum tripolyphosphate composite can significantly improve the corrosion resistance of the coating. The halloysite nanotube has a hollow tubular structure and can act as a physical barrier to prevent corrosive media such as oxygen, moisture and electrolytes from penetrating into the surface of the substrate, thereby delaying the corrosion process; aluminum tripolyphosphate, as a corrosion inhibitor, can decompose under corrosive conditions to produce phosphate ions, which can react with metal ions on the surface of the metal substrate to form a dense protective film to further block the corrosive media.
[0019] 2. The oily coating for stainless steel and aluminum materials prepared in this application has excellent wear resistance and corrosion resistance, a simple preparation method, and is suitable for industrial production.
[0020] 3. The coating prepared in the present application can form a coating with excellent wear resistance and corrosion resistance when applied on stainless steel and broken aluminum materials, and has good adhesion, which can better provide protection for stainless steel and broken aluminum materials. DETAILED DESCRIPTION
[0021] The present application is further described in detail below with reference to the embodiments.
[0022] Preparation Example 1-3 Preparation Example 1 This preparation example provides a lignin nanosphere, and the preparation method comprises the following steps: A1. Mix enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water, and perform ultrasonic dispersion for 20 minutes to completely dissolve the lignin. Then, centrifuge at 8000 rpm for 20 minutes, and take the supernatant to obtain a lignin solution. A2, injecting the prepared lignin solution into ultrapure water to prepare a lignin micro-nanosphere suspension; A3. Add the lignin micro-nanosphere suspension into an autoclave, heat it at 160° C. for 12 hours, and then freeze-dry it to obtain the lignin nano-microspheres.
[0023] Wherein, in step A1, the weight ratio of the enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water is 20:10:1; and in step A2, the volume ratio of the lignin solution to ultrapure water is 1:3.
[0024] Preparation Example 2 This preparation example provides a lignin nanosphere, and the preparation method comprises the following steps: A1. Mix enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water, and perform ultrasonic dispersion for 25 minutes to completely dissolve the lignin. Then, centrifuge at 7500 rpm for 23 minutes, and take the supernatant to obtain a lignin solution. A2, injecting the prepared lignin solution into ultrapure water to prepare a lignin micro-nanosphere suspension; A3. Add the lignin micro-nanosphere suspension into an autoclave, heat it at 170° C. for 11 h, and then freeze-dry it to obtain the lignin nano-microspheres.
[0025] Wherein, in step A1, the weight ratio of the enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water is 22:9:1; and in step A2, the volume ratio of the lignin solution to ultrapure water is 1:4.
[0026] Preparation Example 3 This preparation example provides a lignin nanosphere, and the preparation method comprises the following steps: A1. Mix enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water, and perform ultrasonic dispersion for 30 minutes to completely dissolve the lignin. Then, centrifuge at 7000 rpm for 25 minutes, and take the supernatant to obtain a lignin solution. A2, injecting the prepared lignin solution into ultrapure water to prepare a lignin micro-nanosphere suspension; A3. Add the lignin micro-nanosphere suspension into an autoclave, heat it at 180° C. for 10 h, and then freeze-dry it to obtain the lignin nano-microspheres.
[0027] Wherein, in step A1, the weight ratio of the enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water is 25:8:1; in step A2, the volume ratio of the lignin solution to ultrapure water is 1:5.
[0028] Preparation Example 4 This preparation example provides a halloysite nanotube-aluminum tripolyphosphate composite, and the preparation method includes the following steps: B1, adding a 4 mol / L hydrochloric acid solution to the halloysite nanotubes, heating and stirring for 5 h in a water bath, centrifuging, filtering, washing, and grinding to obtain the halloysite nanotubes etched with hydrochloric acid; B2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step B1, aluminum tripolyphosphate and deionized water, ultrasonically dispersing for 50 minutes, and then vacuum drying the obtained suspension; B3. After vacuum drying, centrifugation is performed to separate the solid phase, and the solid phase is washed, dried, and ground into powder to obtain the halloysite nanotube-corrosion inhibitor composite.
[0029] The weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step B1 is 5:60; the weight ratio of the aluminum tripolyphosphate and deionized water in step B2 to the halloysite nanotubes in step B1 is 6:50:1.
[0030] Preparation Example 5 This preparation example provides a halloysite nanotube-aluminum tripolyphosphate composite, and the preparation method includes the following steps: B1, adding a 4 mol / L hydrochloric acid solution to the halloysite nanotubes, heating and stirring for 5 h in a water bath, centrifuging, filtering, washing, and grinding to obtain the halloysite nanotubes etched with hydrochloric acid; B2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step B1, aluminum tripolyphosphate and deionized water, ultrasonically dispersing for 50 minutes, and then vacuum drying the obtained suspension; B3. After vacuum drying, centrifugation is performed to separate the solid phase, and the solid phase is washed, dried, and ground into powder to obtain the halloysite nanotube-corrosion inhibitor composite.
[0031] The weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step B1 is 6:70; the weight ratio of the aluminum tripolyphosphate and deionized water in step B2 to the halloysite nanotubes in step B1 is 7:55:1.
[0032] Preparation Example 6 This preparation example provides a halloysite nanotube-aluminum tripolyphosphate composite, and the preparation method includes the following steps: B1, adding a 4 mol / L hydrochloric acid solution to the halloysite nanotubes, heating and stirring for 5 h in a water bath, centrifuging, filtering, washing, and grinding to obtain the halloysite nanotubes etched with hydrochloric acid; B2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step B1, aluminum tripolyphosphate and deionized water, ultrasonically dispersing for 50 minutes, and then vacuum drying the obtained suspension; B3. After vacuum drying, centrifugation is performed to separate the solid phase, and the solid phase is washed, dried, and ground into powder to obtain the halloysite nanotube-corrosion inhibitor composite.
[0033] The weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step B1 is 7:80; the weight ratio of the aluminum tripolyphosphate and deionized water in step B2 to the halloysite nanotubes in step B1 is 8:60:1.
[0034] Example 1 The present embodiment provides an oily coating for stainless steel and broken aluminum materials, comprising the following components by weight: 60 parts of epoxy resin, 8 parts of curing agent, 30 parts of organic solvent, 10 parts of nano-silicon dioxide, 5 parts of nano-titanium dioxide, 15 parts of lignin nano-microspheres, 10 parts of halloysite nanotube-aluminum tripolyphosphate complex, 2 parts of dispersant, 1 part of defoaming agent, and 2 parts of leveling agent.
[0035] The preparation method of the oily coating for stainless steel and aluminum materials in this preparation example comprises the following steps: S1, mixing the epoxy resin, organic solvent, defoamer and dispersant uniformly; S2, adding the nano-silicon dioxide, nano-titanium dioxide, lignin nano-microspheres and halloysite nanotube-aluminum tripolyphosphate complex, and stirring at a rotation speed of 750 rpm for 1.2 h; S3, adding the leveling agent and curing agent, stirring for 5 minutes at a rotation speed of 550 rpm, to obtain the oily coating for the stainless steel and aluminum materials.
[0036] The lignin nanospheres used in this embodiment were prepared by Preparation Example 1, the halloysite nanotube-aluminum tripolyphosphate composite was prepared by Preparation Example 4, the curing agent was a modified amine curing agent, the organic solvent was butyl acetate, the dispersant was sodium dodecyl sulfate, the defoaming agent was BYK024, and the leveling agent was a silicone leveling agent.
[0037] Embodiment 2-4 Example 2 The difference between this embodiment and embodiment 1 is that when preparing the oily coating for stainless steel and aluminum materials, the total weight of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 25 parts, and the weight ratio of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 1:1.
[0038] Example 3 The difference between this embodiment and embodiment 1 is that when preparing the oily coating for stainless steel and broken aluminum materials, the total weight of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 25 parts, and the weight ratio of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 1.2:1.
[0039] Example 4 The difference between this embodiment and embodiment 1 is that when preparing the oily coating for stainless steel and broken aluminum materials, the total weight of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 25 parts, and the weight ratio of the lignin nano-microspheres and the halloysite nano-tube-aluminum tripolyphosphate complex is 1.8:1.
[0040] Comparative Examples 1-3 Comparative Example 1 The difference between this comparative example and Example 1 is that the halloysite nanotube-aluminum tripolyphosphate complex is not added when preparing the oily coating for stainless steel and aluminum materials.
[0041] Comparative Example 2 The difference between this comparative example and Example 1 is that no lignin nano-microspheres are added when preparing the oily coating for stainless steel and aluminum materials.
[0042] Comparative Example 3 The difference between this comparative example and Example 1 is that when preparing the oily coating for stainless steel and aluminum materials, no lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complex are added.
[0043] The oily coating for stainless steel and broken aluminum materials prepared in the examples and comparative examples of the present application is used in the field of preparing wear-resistant and anti-corrosion coatings. The prepared oily coating for stainless steel and broken aluminum materials is applied to a pretreated substrate and dried to obtain an anti-corrosion and wear-resistant coating.
[0044] The substrate is one of stainless steel and broken aluminum; the pretreatment includes degreasing, rust removal, and grinding; the drying temperature is 70° C. and the time is 1.2 h.
[0045] The performance of the prepared anti-corrosion coating was tested.
[0046] Experimental testing: The experimental test results of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1.
[0047] Table 1 - Experimental test results of Examples 1-4 and Comparative Examples 1-3 Result analysis: The difference between Examples 2-4 and Example 1 is that when preparing the oily coating for stainless steel and aluminum-breaking materials, the total weight of lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complex is 25 parts, and the weight ratio of lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complex is different. Combined with the experimental test results in Table 1, it can be seen that when the weight ratio of lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complex is 1.5:1, the obtained oily coating for stainless steel and aluminum-breaking materials has good adhesion, excellent wear resistance and corrosion resistance. The difference between Comparative Example 1 and Example 1 is that when preparing the oily coating for stainless steel and aluminum-breaking materials, halloysite nano-tube-aluminum tripolyphosphate complex is not added. The difference between Comparative Example 2 and Example 1 is that when preparing the oily coating for stainless steel and aluminum-breaking materials, lignin nano-microspheres are not added. The difference between Comparative Example 3 and Example 3 is that, when preparing the oily coating for stainless steel and aluminum-breaking materials, no lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complexes were added. Combined with the experimental test results in Table 1, it can be seen that when preparing the oily coating for stainless steel and aluminum-breaking materials, the compound use of lignin nano-microspheres and halloysite nano-tube-aluminum tripolyphosphate complexes can better improve the comprehensive performance of the oily coating for stainless steel and aluminum-breaking materials.
[0048] Embodiment 5-6 The difference between Example 5-6 and Example 3 is that the weight fractions of some components are changed when preparing the oily coating for stainless steel and aluminum. See Table 2 for the differences.
[0049] Table 2 - Differences between Examples 5-6 and Example 3 The experimental test results of Examples 5-6 are shown in Table 3.
[0050] Table 3 - Experimental test results of Examples 5-6 Result analysis: The difference between Example 5-6 and Example 1 is that when preparing the oily coating for stainless steel and broken aluminum materials, the weight proportions of some components are different. Combined with the experimental test results in Table 3, it can be seen that when preparing the oily coating for stainless steel and broken aluminum materials, the oily coating for stainless steel and broken aluminum materials prepared in Example 5 has better comprehensive performance.
[0051] Embodiment 7-8 Example 7 The difference between this embodiment and embodiment 5 is that different preparation parameters of lignin nano-microspheres are used in preparing the oily coating for stainless steel and aluminum materials. The lignin nano-microspheres in this embodiment are prepared by Preparation Example 2.
[0052] Example 8 The difference between this embodiment and embodiment 5 is that different preparation parameters of lignin nano-microspheres are used in preparing the oily coating for stainless steel and aluminum materials. The lignin nano-microspheres in this embodiment are prepared by Preparation Example 3.
[0053] Examples 9-10 Example 9 The difference between this embodiment and embodiment 7 is that when preparing the oily coating for stainless steel and aluminum materials, the preparation parameters of the halloysite nanotube-aluminum tripolyphosphate complex used are different. The halloysite nanotube-aluminum tripolyphosphate complex in this embodiment is prepared by Preparation Example 5.
[0054] Example 10 The difference between this embodiment and embodiment 7 is that when preparing the oily coating for stainless steel and aluminum materials, the preparation parameters of the halloysite nanotube-aluminum tripolyphosphate complex used are different. The halloysite nanotube-aluminum tripolyphosphate complex in this embodiment is prepared by Preparation Example 6.
[0055] The experimental test results of Examples 7-10 are shown in Table 4.
[0056] Table 4 - Experimental test results of Examples 7-10 Result analysis: When preparing oily coatings for stainless steel and aluminum-breaking materials, the lignin nanospheres prepared in Preparation Example 2 and the halloysite nanotube-aluminum tripolyphosphate complex prepared in Preparation Example 5 can better improve the comprehensive performance of oily coatings for stainless steel and aluminum-breaking materials.
[0057] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. An oily paint for stainless steel and aluminum materials, characterized in that: The invention comprises the following components in parts by weight: 60-80 parts of epoxy resin, 8-15 parts of curing agent, 30-50 parts of organic solvent, 10-15 parts of nano silicon dioxide, 5-10 parts of nano titanium dioxide, 8-14 parts of halloysite nanotube-aluminum tripolyphosphate complex, 12-21 parts of lignin nano microspheres, 2-4 parts of dispersant, 1-3 parts of defoaming agent and 2-4 parts of leveling agent.
2. The oily paint for stainless steel and aluminum materials according to claim 1, characterized in that: The preparation method of the lignin nanospheres comprises the following steps: A1. Mix enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water, and disperse by ultrasonication for 20-30 min to completely dissolve the lignin. Then, centrifuge at 7000-8000 rpm for 20-25 min, and take the supernatant to obtain a lignin solution. A2, injecting the prepared lignin solution into ultrapure water to prepare a lignin micro-nanosphere suspension; A3. Add the lignin micro-nanosphere suspension into an autoclave, heat it at 160-180° C. for 10-12 hours, and then freeze-dry it to obtain the lignin nano-microspheres.
3. The oily paint for stainless steel and aluminum materials according to claim 2, characterized in that: In the step A1, the weight ratio of the enzymatically hydrolyzed lignin, γ-valerolactone and ultrapure water is (20-25):(8-10):1; in the step A2, the volume ratio of the lignin solution to ultrapure water is 1:(3-5).
4. The oily paint for stainless steel and aluminum materials according to claim 1, characterized in that: The preparation method of the halloysite nanotube-aluminum tripolyphosphate composite comprises the following steps: B1. Add a hydrochloric acid solution with a concentration of (3-5) mol / L to the halloysite nanotubes, heat and stir in a water bath for 4-6 hours, centrifuge, filter, wash, and grind to obtain the halloysite nanotubes etched with hydrochloric acid; B2, mixing the hydrochloric acid-etched halloysite nanotubes obtained in step B1, aluminum tripolyphosphate and deionized water, ultrasonically dispersing for 40-60 minutes, and then vacuum drying the obtained suspension; B3. After vacuum drying, centrifugation is performed to separate the solid phase, and the solid phase is washed, dried, and ground into powder to obtain the halloysite nanotube-corrosion inhibitor composite.
5. The oily paint for stainless steel and aluminum materials according to claim 4, characterized in that: The weight ratio of the halloysite nanotubes to the hydrochloric acid solution in step B1 is (5-7):(60-80); the weight ratio of the aluminum tripolyphosphate and deionized water in step B2 to the halloysite nanotubes in step B1 is (6-8):(50-60):
1.
6. The oily paint for stainless steel and aluminum materials according to claim 1, characterized in that: The weight ratio of the halloysite nanotube-aluminum tripolyphosphate complex to the lignin nanospheres is 1:(1-1.8).
7. The oily paint for stainless steel and aluminum materials according to claim 1, characterized in that: The curing agent is a modified amine curing agent; the organic solvent is butyl acetate; the dispersant is sodium dodecyl sulfate; the defoaming agent is BYK024; and the leveling agent is an organic silicone leveling agent.
8. A method for preparing an oily coating for stainless steel and aluminum materials according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, mixing the epoxy resin, organic solvent, defoamer and dispersant uniformly; S2, adding the nano-silicon dioxide, nano-titanium dioxide, lignin nano-microspheres and halloysite nanotube-aluminum tripolyphosphate complex, and stirring at a rotation speed of 700-800 rpm for 1-1.5 hours; S3, adding the leveling agent and curing agent, stirring for 4-8 minutes at a rotation speed of 500-600rpm, to obtain the oily coating for the stainless steel and aluminum materials.
9. An application of the oily paint for stainless steel and aluminum materials according to any one of claims 1 to 7 in the field of preparing wear-resistant and anti-corrosion coatings, characterized in that: The oily paint for stainless steel and aluminum materials is coated on the pretreated substrate and dried to obtain an anti-corrosion and wear-resistant coating.
10. The use of the oily paint for stainless steel and aluminum materials according to claim 9 in the field of preparing wear-resistant and anti-corrosion coatings, characterized in that: The substrate is one of stainless steel and aluminum; the pretreatment includes degreasing, rust removal and grinding; the drying temperature is 60-80° C. and the drying time is 1-1.5 hours.
Citation Information
Patent Citations
TDI tripolymer for both bright and matte surfaces as well as preparation method and application thereof
CN112812251A
High-performance graphene marine anticorrosive coating as well as preparation method and application thereof
CN114716889A
Preparation method of lignin micro-nanospheres with adjustable size
CN116731350A
Preparation method of reinforcing steel bar coating loaded with intelligent corrosion inhibitor
CN117816514A
Apparatus for assembly inspection and sorting using vision technology
KR102778660B1
Cited By
Water-based pre-coating primer and preparation method thereof
CN120248725A
Thermosetting composite material with high impact strength and preparation method thereof
CN122011682A