Ether-containing core-shell polyacrylic acid water-based adhesive as well as preparation method and application thereof
By introducing ether bonds and polymerized monomers into the negative electrode adhesive of lithium ion batteries, combined with seed emulsion polymerization technology, an ether-containing core-shell polyacrylic acid water-based adhesive with high adhesion and electrochemical stability was prepared to solve the problem. The problems of low adhesion, poor environmental protection and high cost in the existing technology have made it a good application for the negative electrode of lithium-ion batteries.
Patent Information
- Application Number
- CN202310344165.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-15
AI Technical Summary
Existing adhesives for lithium-ion battery negative electrodes have low adhesion, are not environmentally friendly and are expensive, and cannot meet the comprehensive needs of lithium-ion batteries for adhesion, swelling rate and electrochemical performance.
An ether-containing core-shell polyacrylic acid water-based adhesive is used, and ether bonds are introduced during the polymerization process by selecting basic monomers, functional monomers and cross-linking monomers to prepare adhesives with high adhesion, flexibility and electrochemical stability. polymer, combined with seed emulsion polymerization technology to improve the compatibility and adhesion of latex particles.
It provides high adhesion, good flexibility and electrochemical stability, solves the problems of low adhesion, poor environmental protection and high cost of lithium-ion battery negative electrode adhesives, and has good application prospects.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-based adhesives, and in particular relates to an ether-containing core-shell polyacrylic acid water-based adhesive, and a preparation method and application thereof. Background Art
[0002] As a secondary battery, lithium-ion batteries are widely used in many fields due to their advantages such as high energy conversion rate, high energy density, high rate charge and discharge, no memory effect and environmental friendliness. Polymer adhesives have good bonding properties and can bond various particles together and tightly bond them to the current collector, making them an indispensable part of lithium-ion batteries. In addition to high adhesion, high-performance adhesives also need to have the following characteristics: good flexibility, electrolyte resistance, compactness, chemical and electrochemical stability, low cost and environmental protection.
[0003] At present, the adhesives used in lithium-ion batteries in the industry are mainly divided into three categories: polyvinylidene fluoride (PVDF), styrene-butadiene rubber latex and carboxymethyl cellulose (SBR / CMC), and polyacrylic acid (PAA). PVDF has the advantages of good adhesion to aluminum foil and strong resistance to electrochemical corrosion, but its adhesion to copper foil is poor, and PVDF has a large molecular weight and no hydrophilic groups. It is commonly dispersed and dissolved with N-methylpyrrolidone (NMP), but NMP solvent is sensitive to moisture, toxic, and volatilizes to pollute the environment; SBR / CMC adhesive has poor process performance and harsh conditions, and is greatly affected by factors such as stirring, pH, and electrode material ratio. At the same time, the prices of both PVDF and SBR / CMC are relatively high. PAA adhesive has the advantages of strong adhesion, good stability, low price, and environmental protection, and is now a hot research topic for negative electrode adhesives. However, ordinary PAA adhesives cannot meet the comprehensive requirements for negative electrode sheets.
[0004] Therefore, in the art, the PAA adhesive needs to be modified to simultaneously meet the requirements for adhesion, swelling rate and electrochemical performance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an ether-containing core-shell polyacrylic acid aqueous adhesive and its preparation method and application. The ether-containing core-shell polyacrylic acid aqueous adhesive of the present invention has high bonding force, good flexibility and electrochemical stability, and has good application prospects in lithium ion battery negative electrode sheets.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] On the one hand, the present invention provides an ether-containing core-shell polyacrylic acid aqueous adhesive, wherein the ether-containing core-shell polyacrylic acid aqueous adhesive is a polymer having a core-shell structure obtained by polymerizing monomers, wherein the polymerizing monomers include a basic monomer, a first functional monomer, a second functional monomer and a cross-linking monomer;
[0008] The basic monomer is selected from any one or a combination of at least two of methyl acrylate, methyl methacrylate, ethyl acrylate, styrene, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acrylate, lauric methacrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate; the first functional monomer is selected from any one or a combination of at least two of acrylic acid, methacrylic acid, acrylonitrile, acrylamide, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate; the cross-linking monomer is selected from any one or a combination of at least two of diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate or silane coupling agent.
[0009] In the present invention, by selecting basic monomers, first functional monomers, second functional monomers and cross-linking monomers, ether bonds are introduced into the polyacrylic acid structure during the monomer polymerization process, so that the prepared ether-containing core-shell polyacrylic acid water-based adhesive has higher bonding force, better flexibility and electrochemical stability.
[0010] Preferably, the first functional monomer is selected from any one or a combination of at least two of ethoxyethoxyethyl acrylate, methoxy polyethylene glycol acrylate, polyethylene glycol acrylate or polyethylene glycol diacrylate.
[0011] Preferably, the polymerized monomers of the core include the following components in parts by weight: 12.5 to 80 parts (e.g., 12.5, 15, 20, 30, 40, 50, 60, 70 or 80 parts) of a basic monomer, 0.25 to 30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of a first functional monomer, 0.25 to 30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of a second functional monomer and 0.25 to 15 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10 or 15 parts) of a cross-linking monomer.
[0012] Preferably, the polymerized monomers of the shell include the following components in percentage by weight: 10 to 75 parts (e.g., 10, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 or 75 parts) of basic monomers, 0.2 to 30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of first functional monomers, 0.2 to 30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of second functional monomers and 0.1 to 15 parts (e.g., 0.2, 0.5, 1, 3, 5, 8, 10 or 15 parts) of cross-linking monomers.
[0013] In the present invention, by controlling the composition ratio of the polymerized monomers of the core and shell, core-shell latex particles with different structural morphologies can be obtained, the compatibility and adhesion between the two can be increased, and the processing performance can be improved.
[0014] Preferably, the ether-containing core-shell polyacrylic acid aqueous adhesive is obtained by emulsion polymerization.
[0015] On the other hand, the present invention provides a method for preparing the ether-containing core-shell polyacrylic acid aqueous adhesive as described above, the preparation method comprising the following steps:
[0016] (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a kettle bottom reaction liquid and an initiator solution;
[0017] (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting;
[0018] (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react;
[0019] (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the ether-containing core-shell polyacrylic acid aqueous adhesive.
[0020] In the present invention, the ether-containing core-shell polyacrylic acid aqueous adhesive is obtained by emulsion polymerization in the form of seed emulsion polymerization.
[0021] Preferably, the seed emulsion polymerization of the present invention can increase the compatibility and adhesion of the obtained shell structure particles, and can also improve the mechanical properties; the latex particles obtained by the addition sequence and conditions of the present invention are stronger than ordinary emulsion polymerization in terms of rheology, minimum film forming temperature, glass transition temperature, adhesion, processability, etc. The seed emulsion polymerization can effectively control the diameter and distribution of the latex particles. Directly adding the core pre-emulsion liquid and the initiator to react will make the obtained latex particle size very small, which is not conducive to its adhesion, processing and mechanical properties.
[0022] Preferably, the core pre-emulsion comprises basic monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water.
[0023] Preferably, the core pre-emulsion comprises 12.25 to 65 parts (e.g., 13, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60 or 65 parts) of basic monomers, 0.245 to 25 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20 or 25 parts) of second functional monomers and 0.25 to 15 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10 or 15 parts) of cross-linking monomers.
[0024] Preferably, the amount of emulsifier in the core pre-emulsion is 0.25%-4% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example 0.25%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.
[0025] Preferably, the amount of deionized water in the core pre-emulsion is 10% to 80% of the total weight of the basic monomers, second functional monomers and cross-linking monomers in the core pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0026] Preferably, the core pre-emulsified seed emulsion comprises a basic monomer, a second functional monomer, an emulsifier and deionized water.
[0027] Preferably, the core pre-emulsified seed emulsion contains 0.25-18 parts (e.g., 0.3 parts, 0.5 parts, 1 parts, 3 parts, 5 parts, 8 parts, 10 parts, 15 parts or 18 parts) of basic monomers and 0.005-8 parts (e.g., 0.008 parts, 0.01 parts, 0.1 parts, 0.2 parts, 0.5 parts, 1 parts, 3 parts, 5 parts or 8 parts) of second functional monomers.
[0028] Preferably, the amount of emulsifier in the core pre-emulsified seed emulsion is 0.005%-1% of the total weight of the basic monomers and the second functional monomers in the seed emulsion of the core pre-emulsified liquid, for example 0.005%, 0.008%, 0.01%, 0.1%, 0.3%, 0.5%, 0.8% or 1%.
[0029] Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10% to 80% of the total weight of the basic monomers, secondary functional monomers and cross-linking monomers in the seed emulsion of the core pre-emulsified liquid, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0030] Preferably, the shell pre-emulsion comprises basic monomers, first functional monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water.
[0031] Preferably, the shell pre-emulsion includes 10-75 parts (e.g., 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70 or 75 parts) of basic monomers, 0.2-30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of first functional monomers, 0.2-30 parts (e.g., 0.3, 0.5, 1, 3, 5, 8, 10, 15, 20, 25 or 30 parts) of second functional monomers and 0.1-15 parts (e.g., 0.2, 0.5, 1, 3, 5, 8, 10 or 15 parts) of cross-linking monomers.
[0032] Preferably, the amount of emulsifier in the shell pre-emulsion is 0.2%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion, for example 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5% or 4%.
[0033] Preferably, the amount of deionized water in the shell pre-emulsion is 10% to 80% of the total weight of the basic monomers, the first functional monomers, the second functional monomers and the cross-linking monomers in the core pre-emulsion, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0034] Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer.
[0035] Preferably, the content of each component in the reaction liquid at the bottom of the kettle is 0.1-3 parts (for example, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts or 3 parts) of emulsifier, 50-120 parts (for example, 50 parts, 60 parts, 70 parts, 75 parts, 80 parts, 90 parts, 100 parts, 110 parts or 120 parts) of deionized water, and 0.25-1 parts (for example, 0.25 parts, 0.3 parts, 0.5 parts, 0.7 parts or 1 parts) of buffer.
[0036] Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof.
[0037] Preferably, the buffer is sodium bicarbonate, ammonia water, ammonium bicarbonate, or sodium hydroxide.
[0038] Preferably, the initiator solution comprises an initiator and deionized water.
[0039] Preferably, the amount of deionized water in the initiator solution is 1-20 parts, for example, 1 part, 3 parts, 5 parts, 8 parts, 10 parts, 13 parts, 15 parts, 18 parts or 20 parts, relative to 1 part by weight of the initiator.
[0040] Preferably, the initiator is selected from inorganic peroxide initiators.
[0041] Preferably, the initiator is selected from any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof.
[0042] Preferably, the reaction in steps (2) to (4) is carried out under stirring, and the stirring speed is 100-500 r / min (for example, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min, 350 r / min, 400 r / min, 450 r / min, 500 r / min).
[0043] Preferably, before adding the pre-emulsified seed emulsion in step (2), the reaction liquid at the bottom of the kettle is added to a reactor at 40-75°C (e.g., 40°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C, 70°C or 75°C).
[0044] Preferably, the heating in step (2) is to 75-85°C, for example, 75°C, 78°C, 80°C, 83°C or 85°C.
[0045] Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 3-84 times, for example, 3 times, 5 times, 8 times, 10 times, 20 times, 30 times, 40 times, 45 times, 50 times, 60 times, 70 times, 80 times or 84 times, of the pre-emulsified seed emulsion.
[0046] Preferably, the amount of the initiator solution added in step (2) is 0.06%-15% by weight of the core pre-emulsified seed emulsion, for example 0.06%, 0.8%, 1%, 2%, 4%, 6%, 8%, 10%, 13% or 15%.
[0047] Preferably, the reaction time of step (2) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.
[0048] Preferably, the weight ratio of the core pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 1:0.15-1, for example, 1:0.15, 1:0.3, 1:0.5, 1:0.7, 1:0.8 or 1:1.
[0049] Preferably, the amount of the initiator solution added in step (3) is 0.0045%-15% by weight of the core pre-emulsion, for example 0.0045%, 0.2%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13% or 15%.
[0050] Preferably, the reaction temperature in step (3) is 75-85°C, such as 75°C, 78°C, 80°C, 83°C or 85°C.
[0051] Preferably, the reaction time of step (3) is 10-30 min, for example, 10 min, 13 min, 15 min, 18 min, 20 min, 23 min, 25 min, 28 min or 30 min.
[0052] Preferably, the weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3, for example, 1:0.25, 1:0.3, 1:0.5, 1:0.8, 1:1, 1:1.5, 1:1.8, 1:2, 1:2.5, 1:2.8 or 1:3.
[0053] Preferably, the amount of the initiator solution added in step (4) is 0.006%-15% by weight of the shell pre-emulsion, for example 0.006%, 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 13% or 15%.
[0054] Preferably, the reaction temperature in step (4) is 80-90°C, such as 80°C, 83°C, 85°C, 88°C or 90°C.
[0055] Preferably, the reaction time of step (4) is 0.5-2.5 h, for example 0.5 h, 0.8 h, 1 h, 1.5 h, 1.8 h, 2 h, 2.3 h or 2.5 h.
[0056] In the present invention, after the reaction in step (4) is completed, the temperature is lowered to 60-70°C (for example, 60°C, 63°C, 65°C, 68°C or 70°C), a residual monomer eliminator is added, and then the temperature is lowered to below 50°C (for example, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 10°C, etc.), the pH is adjusted to 7-8 (for example, 7, 7.3, 7.5, 7.8 or 8), and the material is filtered to obtain the ether-containing core-shell polyacrylic acid aqueous adhesive.
[0057] Preferably, the residual monomer eliminating agent is bleaching powder and tert-butyl peroxide.
[0058] Preferably, the reagent used to adjust the pH is any one of ammonia water, sodium hydroxide, lithium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof.
[0059] In the present invention, by designing the monomer types and mass ratios in the core and shell pre-emulsions, an ether-containing core-shell polyacrylic acid aqueous adhesive that is hard inside and soft outside is prepared. By introducing ether bonds, carboxylic acids and carboxylates, and ester groups into the adhesive, the prepared core-shell polyacrylic acid aqueous adhesive has flexibility, electrochemical stability, and good adhesion, and has good application prospects in lithium-ion battery negative electrode plates.
[0060] On the other hand, the present invention provides a negative electrode plate for a lithium ion battery, wherein the negative electrode plate for the lithium ion battery comprises the ether-containing core-shell polyacrylic acid aqueous adhesive as described above.
[0061] In another aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the lithium ion battery negative electrode sheet as described above.
[0062] Compared with the prior art, the present invention has the following beneficial effects:
[0063] The ether-containing core-shell polyacrylic acid aqueous adhesive provided by the present invention has high bonding force, good flexibility and electrochemical stability, solves the problems of low bonding, environmental pollution and high price of current adhesives for negative electrodes of lithium ion batteries, and has good application prospects in negative electrode plates of lithium ion batteries. DETAILED DESCRIPTION
[0064] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0065] Example 1
[0066] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0067] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0068] Nuclear pre-emulsion: dissolve 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.229 parts of polyoxyethylene octylphenol ether-10 in 17 parts of deionized water, then sequentially add 19.76 parts of methyl methacrylate, 14.45 parts of butyl acrylate, 3.62 parts of isooctyl acrylate, 0.85 parts of acrylonitrile, 0.212 parts of acrylamide, 1.275 parts of acrylic acid, 0.425 parts of methacrylic acid, and 1.062 parts of hydroxyethyl methacrylate for emulsification, add 2 parts of ethoxylated trimethylolpropane triacrylate into the nuclear pre-emulsion for uniform emulsification;
[0069] Seed emulsion: 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.041 parts of polyoxyethylene octylphenol ether-10 are dissolved in 3 parts of deionized water, and then 3.49 parts of methyl methacrylate, 2.55 parts of butyl acrylate, 0.628 parts of isooctyl acrylate, 0.15 parts of acrylonitrile, 0.038 parts of acrylamide, 0.225 parts of acrylic acid, 0.075 parts of methacrylic acid, and 0.188 parts of hydroxyethyl methacrylate are added in sequence for emulsification to obtain a seed emulsion;
[0070] Shell pre-emulsion: 0.53 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.27 parts of polyoxyethylene octylphenol ether-10 are dissolved in 20 parts of deionized water, and then 20.5 parts of methyl methacrylate, 20 parts of butyl acrylate, 5 parts of isooctyl acrylate, 1 part of acrylonitrile, 0.25 parts of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1.25 parts of hydroxyethyl methacrylate, 1 part of glycidyl methacrylate, and 3 parts of ethoxyethoxyethyl acrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0071] A bottom reaction liquid: 0.27 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0072] Initiator solution: Add 0.6 parts of ammonium persulfate to 6 parts of deionized water to obtain an initiator aqueous solution.
[0073] 60.9 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 120rpm. 10.4 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.6 parts of the initiator solution were added, and after reacting for 15 minutes, 61.3 parts of the core pre-emulsion and 2.4 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 74.8 parts of the shell pre-emulsion and 3 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.45 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0074] Example 2
[0075] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0076] (1) Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0077] Nuclear pre-emulsion: dissolve 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.229 parts of polyoxyethylene octylphenol ether-10 in 17 parts of deionized water, then sequentially add 19.75 parts of methyl methacrylate, 14.45 parts of butyl acrylate, 3.622 parts of isooctyl acrylate, 0.85 parts of acrylonitrile, 0.212 parts of acrylamide, 1.275 parts of acrylic acid, 0.425 parts of methacrylic acid, and 1.062 parts of hydroxyethyl methacrylate for emulsification, add 2 parts of ethoxylated trimethylolpropane triacrylate to the nuclear pre-emulsion for uniform emulsification;
[0078] Seed emulsion: 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.041 parts of polyoxyethylene octylphenol ether-10 are dissolved in 3 parts of deionized water, and then 3.49 parts of methyl methacrylate, 2.55 parts of butyl acrylate, 0.628 parts of isooctyl acrylate, 0.15 parts of acrylonitrile, 0.038 parts of acrylamide, 0.225 parts of acrylic acid, 0.075 parts of methacrylic acid, and 0.188 parts of hydroxyethyl methacrylate are added in sequence for emulsification to obtain a seed emulsion;
[0079] Shell pre-emulsion: 0.53 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.27 parts of polyoxyethylene octylphenol ether-10 are dissolved in 20 parts of deionized water, and then 20.5 parts of methyl methacrylate, 20 parts of butyl acrylate, 5 parts of isooctyl acrylate, 1 part of acrylonitrile, 0.25 parts of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1.25 parts of hydroxyethyl methacrylate, and 5 parts of ethoxyethoxyethyl acrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0080] A bottom reaction liquid: 0.27 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0081] Initiator solution: Add 0.6 parts of ammonium persulfate to 6 parts of deionized water to obtain an initiator aqueous solution.
[0082] 60.9 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 120rpm. 10.465 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.6 parts of the initiator solution were added, and after reacting for 15 minutes, 61.3 parts of the core pre-emulsion and 2.4 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 75.8 parts of the shell pre-emulsion and 3 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to below 50°C, and the pH was adjusted to 7.45 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0083] Example 3
[0084] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0085] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0086] Nuclear pre-emulsion: dissolve 1 part of sodium dodecyl sulfate and 0.5 part of polyoxyethylene octylphenol ether-10 in 25 parts of deionized water, then add 20 parts of methyl methacrylate, 16 parts of n-butyl methacrylate, 4 parts of n-octyl acrylate, 5 parts of acrylonitrile, 1 part of acrylamide, 6 parts of acrylic acid, 2 parts of methacrylic acid, and 2 parts of 4-hydroxybutyl acrylate in sequence for emulsification, add 4 parts of glycidyl methacrylate into the nuclear pre-emulsion and emulsify evenly;
[0087] Seed emulsion: dissolve 0.1 parts of sodium dodecyl sulfate and 0.05 parts of polyoxyethylene octylphenol ether-10 in 2.5 parts of deionized water, and then sequentially add 2 parts of methyl methacrylate, 1.6 parts of n-butyl methacrylate, 0.4 parts of n-octyl acrylate, 0.5 parts of acrylonitrile, 0.1 parts of acrylamide, 0.6 parts of acrylic acid, 0.2 parts of methacrylic acid, and 0.2 parts of 4-hydroxybutyl acrylate for emulsification to obtain a seed emulsion;
[0088] Shell pre-emulsion: dissolve 1 part of sodium dodecyl sulfate and 0.5 part of polyoxyethylene octylphenol ether-10 in 30 parts of deionized water, and then add 10 parts of methyl methacrylate, 30 parts of n-butyl methacrylate, 10 parts of n-octyl acrylate, 6 parts of acrylonitrile, 2 parts of acrylamide, 6 parts of acrylic acid, 2 parts of methacrylic acid, 2 parts of 4-hydroxybutyl acrylate, 2 parts of diacetone acrylamide, and 10 parts of methoxy polyethylene glycol acrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0089] Still bottom reaction liquid: 0.5 parts of sodium dodecyl sulfate and 0.25 parts of polyoxyethylene octylphenol ether-10 are dissolved in 80 parts of deionized water, and then 0.7 parts of ammonium bicarbonate are added to obtain a still bottom reaction liquid;
[0090] Initiator solution: Add 0.6 parts of potassium persulfate into 20 parts of deionized water to obtain an initiator aqueous solution.
[0091] 81.45 parts of the bottom reaction liquid were added to a 50°C reactor at a speed of 150 rpm. 8.25 parts of the seed emulsion were added to the reactor, heated to 75°C, 0.89 parts of the initiator solution were added, and after reacting for 15 minutes, 86.5 parts of the core pre-emulsion and 8.96 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 111.5 parts of the shell pre-emulsion and 10.75 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 80°C for 2.3 hours. After the reaction was completed, the temperature was lowered to 70°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 50°C. The pH was adjusted to 7.68 using 25% mass percent ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0092] Example 4
[0093] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0094] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0095] Core pre-emulsion: dissolve 2 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 in 30 parts of deionized water, then add 25 parts of styrene, 18 parts of isobutyl methacrylate, 10 parts of lauric acid acrylate, 8 parts of acrylonitrile, 2 parts of acrylamide, 4 parts of acrylic acid, 2 parts of methacrylic acid, and 4 parts of hydroxypropyl methacrylate in sequence for emulsification, add 6 parts of divinylbenzene into the core pre-emulsion and emulsify evenly;
[0096] Seed emulsion: dissolve 0.4 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 0.2 parts of polyoxyethylene octylphenol ether-10 in 6 parts of deionized water, and then add 5 parts of styrene, 3.6 parts of isobutyl methacrylate, 2 parts of lauric acid acrylate, 1.6 parts of acrylonitrile, 0.4 parts of acrylamide, 0.8 parts of acrylic acid, 0.4 parts of methacrylic acid, and 0.8 parts of hydroxypropyl methacrylate in sequence for emulsification to obtain a seed emulsion;
[0097] Shell pre-emulsion: dissolve 2 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 in 40 parts of deionized water, and then add 15 parts of styrene, 35 parts of isobutyl methacrylate, 15 parts of lauric acid acrylate, 8 parts of acrylonitrile, 2 parts of acrylamide, 4 parts of acrylic acid, 2 parts of methacrylic acid, 4 parts of hydroxypropyl methacrylate, 5 parts of diacetone acrylamide, and 10 parts of methoxy polyethylene glycol acrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0098] Still bottom reaction liquid: dissolve 1 part of allyloxy fatty alcohol oxyethylene ether ammonium sulfate and 1 part of polyoxyethylene octylphenol ether-10 in 100 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0099] Initiator solution: Add 0.6 parts of ammonium persulfate into 13 parts of deionized water to obtain an initiator aqueous solution.
[0100] 103 parts of the bottom reaction liquid were added to a reactor at 65°C, with a rotation speed of 200rpm. 21.2 parts of the seed emulsion were added to the reactor, heated to 78°C, 1.23 parts of the initiator solution were added, and after reacting for 20 minutes, 112 parts of the core pre-emulsion and 6.15 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 18 minutes, 143 parts of the shell pre-emulsion and 8.21 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 85°C for 1.8 hours. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.68 with sodium hydroxide, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0101] Example 5
[0102] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0103] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0104] Nuclear pre-emulsion: dissolve 2 parts of sodium dodecylbenzene sulfonate and 2 parts of polyoxyethylene octylphenol ether-10 in 30 parts of deionized water, then add 13 parts of styrene, 17 parts of methyl methacrylate, 15 parts of butyl acrylate, 13 parts of lauric acid methacrylate, 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, and 4 parts of hydroxypropyl methacrylate in sequence for emulsification, add 6 parts of ethoxylated trimethylolpropane triacrylate into the nuclear pre-emulsion for uniform emulsification;
[0105] Seed emulsion: 0.4 parts of sodium dodecylbenzene sulfonate and 0.4 parts of polyoxyethylene octylphenol ether-10 were dissolved in 7.5 parts of deionized water, and then 3.25 parts of styrene, 4.25 parts of methyl methacrylate, 3.75 parts of butyl acrylate, 3.25 parts of lauric acid methacrylate, 1.25 parts of acrylamide, 2 parts of acrylic acid, 1 part of methacrylic acid, and 1 part of hydroxypropyl methacrylate were added in sequence for emulsification to obtain a seed emulsion;
[0106] Shell pre-emulsion: dissolve 2 parts of sodium dodecylbenzene sulfonate and 2 parts of polyoxyethylene octylphenol ether-10 in 40 parts of deionized water, and then add 10 parts of styrene, 15 parts of methyl methacrylate, 30 parts of butyl acrylate, 20 parts of lauric acid methacrylate, 5 parts of acrylamide, 8 parts of acrylic acid, 4 parts of methacrylic acid, 4 parts of hydroxypropyl methacrylate, 1.5 parts of aziridine, 1 part of silane coupling agent, and 5 parts of polyethylene glycol diacrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0107] Still bottom reaction liquid: 1.5 parts of sodium dodecylbenzene sulfonate and 1.5 parts of polyoxyethylene octylphenol ether-10 are dissolved in 120 parts of deionized water, and then 0.25 parts of sodium hydroxide are added to obtain a still bottom reaction liquid;
[0108] Initiator solution: Add 0.6 parts of ammonium persulfate into 15 parts of deionized water to obtain an initiator aqueous solution.
[0109] 123.25 parts of the bottom reaction liquid were added to a reactor at 75°C, with a rotation speed of 250rpm. 28.05 parts of the seed emulsion were added to the reactor, heated to 83°C, 1.4 parts of the initiator solution were added, and after reacting for 25 minutes, 119 parts of the core pre-emulsion and 12 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 23 minutes, 147.5 parts of the shell pre-emulsion and 2.2 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 88°C for 0.5h. After the reaction was completed, the temperature was lowered to 60°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 10°C. The pH was adjusted to 7.68 using lithium hydroxide, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0110] Example 6
[0111] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0112] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0113] Nuclear pre-emulsion: Disodium succinate nonylphenol polyoxyethylene ether sulfonate (3 parts) was dissolved in 25 parts of deionized water, followed by sequential addition of 28 parts of styrene, 18 parts of butyl acrylate, 3 parts of isooctyl acrylate, 5 parts of acrylamide, 2 parts of methacrylic acid, and 10 parts of hydroxyethyl methacrylate for emulsification, and 3 parts of N-hydroxymethyl acrylamide was added to the nuclear pre-emulsion for uniform emulsification;
[0114] Seed emulsion: dissolve 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 4 parts of deionized water, and then sequentially add 4.2 parts of styrene, 2.7 parts of butyl acrylate, 0.45 parts of isooctyl acrylate, 0.75 parts of acrylamide, 0.3 parts of methacrylic acid, and 1.5 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0115] Shell pre-emulsion: dissolve 2.5 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 25 parts of deionized water, and then add 25 parts of styrene, 35 parts of butyl acrylate, 8 parts of isooctyl acrylate, 4 parts of acrylamide, 8 parts of methacrylic acid, 3 parts of glycidyl methacrylate, and 15 parts of ethoxyethoxyethyl acrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0116] Still bottom reaction liquid: dissolve 1 part of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate in 90 parts of deionized water, and then add 0.5 parts of sodium bicarbonate to obtain a still bottom reaction liquid;
[0117] Initiator solution: Add 0.6 parts of ammonium persulfate into 10 parts of deionized water to obtain an initiator aqueous solution.
[0118] 91.5 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 300rpm. 14.35 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.742 parts of the initiator solution were added, and after reacting for 15 minutes, 97 parts of the core pre-emulsion and 6 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 125.5 parts of the shell pre-emulsion and 3.858 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.54 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0119] Example 7
[0120] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0121] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0122] Core pre-emulsion: 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate are dissolved in 20 parts of deionized water, followed by the addition of 25 parts of methyl methacrylate, 14 parts of isooctyl acrylate, 5 parts of acrylamide, 4 parts of acrylic acid, and 8 parts of hydroxyethyl methacrylate in sequence for emulsification, and 4 parts of ethoxylated trimethylolpropane triacrylate are added to the core pre-emulsion for uniform emulsification;
[0123] Seed emulsion: dissolve 0.45 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 2.5 parts of deionized water, and then add 5 parts of methyl methacrylate, 2.8 parts of isooctyl acrylate, 1 part of acrylamide, 0.8 parts of acrylic acid, and 1.6 parts of hydroxyethyl methacrylate in sequence for emulsification to obtain a seed emulsion;
[0124] Shell pre-emulsion: dissolve 2.5 parts of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 30 parts of deionized water, and then add 10 parts of styrene, 30 parts of lauric acid methacrylate, 4 parts of acrylonitrile, 8 parts of methacrylic acid, 2 parts of diacetone acrylamide, and 8 parts of methoxy polyethylene glycol acrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0125] Still bottom reaction liquid: dissolve 1 part of allyloxy fatty alcohol oxyethylene ether ammonium sulfate in 70 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0126] Initiator solution: Add 0.6 parts of ammonium persulfate into 8 parts of deionized water to obtain an initiator aqueous solution.
[0127] 72 parts of the bottom reaction liquid were added to a reactor at 55°C, with a rotation speed of 350rpm. 14.15 parts of the seed emulsion were added to the reactor, heated to 82°C, 0.43 parts of the initiator solution were added, and after reacting for 15 minutes, 82.5 parts of the core pre-emulsion and 3 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 94.5 parts of the shell pre-emulsion and 5.17 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 86°C for 1.5 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 40°C. The pH was adjusted to 7.71 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0128] Example 8
[0129] In this embodiment, a method for preparing an ether-containing core-shell polyacrylic acid aqueous adhesive is provided, and the preparation method comprises the following steps:
[0130] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0131] Core pre-emulsion: Disodium succinate nonylphenol polyoxyethylene ether sulfonate was added in 30 parts of deionized water, followed by 10 parts of methyl methacrylate, 18 parts of butyl acrylate, 10 parts of acrylonitrile, 5 parts of acrylic acid, and 6 parts of hydroxyethyl methacrylate in sequence for emulsification, and 3 parts of ethoxylated trimethylolpropane triacrylate was added to the core pre-emulsion for uniform emulsification;
[0132] Seed emulsion: dissolve 0.5 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 3 parts of deionized water, and then sequentially add 1 part of methyl methacrylate, 1.8 parts of butyl acrylate, 1 part of acrylonitrile, 0.5 parts of acrylic acid, and 0.6 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0133] Shell pre-emulsion: dissolve 2 parts of disodium succinate nonylphenol polyoxyethylene ether sulfonate in 35 parts of deionized water, and then add 10 parts of styrene, 30 parts of isooctyl acrylate, 4 parts of acrylamide, 8 parts of methacrylic acid, 2 parts of 4-hydroxybutyl acrylate, and 5 parts of ethoxyethoxyethyl acrylate in sequence for emulsification to obtain a shell pre-emulsion;
[0134] Still bottom reaction liquid: dissolve 0.5 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate in 60 parts of deionized water, and then add 1 part of ammonia water to obtain a still bottom reaction liquid;
[0135] Initiator solution: Add 0.6 parts of ammonium persulfate into 9 parts of deionized water to obtain an initiator aqueous solution.
[0136] 61.5 parts of the bottom reaction liquid were added to a 50°C reactor at a speed of 150 rpm. 8.4 parts of the seed emulsion were added to the reactor, heated to 81°C, 0.5 parts of the initiator solution were added, and after reacting for 15 minutes, 126 parts of the core pre-emulsion and 4.5 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 95 parts of the shell pre-emulsion and 4.6 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 85°C for 1.2 hours. After the reaction was completed, the temperature was lowered to 67°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 30°C. The pH was adjusted to 7.71 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0137] Comparative Example 1
[0138] In this comparative example, unlike Example 1, ethoxyethoxyethyl acrylate was not included in the shell pre-emulsion.
[0139] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0140] Nuclear pre-emulsion: 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.229 parts of polyoxyethylene octylphenol ether-10 are dissolved in 17 parts of deionized water, and then 19.76 parts of methyl methacrylate, 14.45 parts of butyl acrylate, 3.622 parts of isooctyl acrylate, 0.85 parts of acrylonitrile, 0.212 parts of acrylamide, 1.275 parts of acrylic acid, 0.425 parts of methacrylic acid, and 1.062 parts of hydroxyethyl methacrylate are added in sequence for emulsification, and 2 parts of ethoxylated trimethylolpropane triacrylate are added to the nuclear pre-emulsion for uniform emulsification;
[0141] Seed emulsion: Dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.041 parts of polyoxyethylene octylphenol ether-10 in 3 parts of deionized water, then add 3.49 parts of methyl methacrylate, 2.55 parts of butyl acrylate, 0.628 parts of isooctyl acrylate, 0.15 parts of acrylonitrile, 0.038 parts of acrylamide, 0.225 parts of acrylic acid, 0.075 parts of methacrylic acid, and 0.188 parts of hydroxyethyl methacrylate in sequence for emulsification to obtain a core pre-emulsified seed emulsion.
[0142] Shell pre-emulsion: 0.53 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.27 parts of polyoxyethylene octylphenol ether-10 are dissolved in 20 parts of deionized water, and then 20.5 parts of methyl methacrylate, 20 parts of butyl acrylate, 5 parts of isooctyl acrylate, 1 part of acrylonitrile, 0.25 parts of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1.25 parts of hydroxyethyl methacrylate and 1 part of glycidyl methacrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0143] A bottom reaction liquid: 0.27 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0144] Initiator solution: Add 0.6 parts of ammonium persulfate to 6 parts of deionized water to obtain an initiator aqueous solution.
[0145] 60.9 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 120rpm. 10.4 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.6 parts of the initiator solution were added, and after reacting for 15 minutes, 61.3 parts of the core pre-emulsion and 2.4 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 74.8 parts of the shell pre-emulsion and 3 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.45 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0146] Comparative Example 2
[0147] In this comparative example, what is different from Example 1 is that the traditional seed emulsion polymerization is not prepared into core-shell emulsion polymerization.
[0148] Preparation of pre-emulsion, seed emulsion, bottom reaction liquid and initiator solution.
[0149] Pre-emulsion: dissolve 0.98 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.499 parts of polyoxyethylene octylphenol ether-10 in 37 parts of deionized water, then sequentially add 40.26 parts of methyl methacrylate, 34.45 parts of butyl acrylate, 8.62 parts of isooctyl acrylate, 1.85 parts of acrylonitrile, 0.462 parts of acrylamide, 2.775 parts of acrylic acid, 0.925 parts of methacrylic acid, 2.312 parts of hydroxyethyl methacrylate, 1 part of glycidyl methacrylate, 3 parts of ethoxyethoxyethyl acrylate, and 2 parts of ethoxylated trimethylolpropane triacrylate into the pre-emulsion, and emulsify evenly;
[0150] Seed emulsion: Dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.041 parts of polyoxyethylene octylphenol ether-10 in 3 parts of deionized water, then add 3.49 parts of methyl methacrylate, 2.55 parts of butyl acrylate, 0.628 parts of isooctyl acrylate, 0.15 parts of acrylonitrile, 0.038 parts of acrylamide, 0.225 parts of acrylic acid, 0.075 parts of methacrylic acid, and 0.188 parts of hydroxyethyl methacrylate in sequence for emulsification to obtain a seed emulsion.
[0151] A bottom reaction liquid: 0.27 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0152] Initiator solution: Add 0.6 parts of ammonium persulfate to 6 parts of deionized water to obtain an initiator aqueous solution.
[0153] 60.9 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 120rpm. 10.465 parts of the seed emulsion were added to the reactor, the temperature was raised to 80°C, 0.6 parts of the initiator solution were added, and after the reaction for 15 minutes, 136.1 parts of the pre-emulsion and 5.4 parts of the initiator solution were added dropwise, and after the addition was completed, the reaction was kept at 87°C for 1 hour, and after the insulation was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 40°C, and the pH was adjusted to 7.24 with 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing polyacrylic acid water-based adhesive.
[0154] Comparative Example 3
[0155] In this comparative example, unlike Example 1, a core-shell emulsion polymerization having a composition opposite to that of the original core-shell was provided.
[0156] Preparation of core pre-emulsion, seed emulsion, shell pre-emulsion, kettle bottom reaction liquid and initiator solution.
[0157] Nuclear pre-emulsion: dissolve 0.45 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.229 parts of polyoxyethylene octylphenol ether-10 in 17 parts of deionized water, then sequentially add 17.43 parts of methyl methacrylate, 17 parts of butyl acrylate, 4.25 parts of isooctyl acrylate, 0.85 parts of acrylonitrile, 0.212 parts of acrylamide, 1.275 parts of acrylic acid, 0.425 parts of methacrylic acid, 1.062 parts of hydroxyethyl methacrylate, 3 parts of ethoxyethoxyethyl acrylate, and 1 part of glycidyl methacrylate into the nuclear pre-emulsion, and emulsify evenly;
[0158] Seed emulsion: dissolve 0.08 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.041 parts of polyoxyethylene octylphenol ether-10 in 3 parts of deionized water, and then sequentially add 3.075 parts of methyl methacrylate, 3 parts of butyl acrylate, 0.75 parts of isooctyl acrylate, 0.15 parts of acrylonitrile, 0.038 parts of acrylamide, 0.225 parts of acrylic acid, 0.075 parts of methacrylic acid, and 0.188 parts of hydroxyethyl methacrylate for emulsification to obtain a seed emulsion;
[0159] Shell pre-emulsion: 0.53 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.27 parts of polyoxyethylene octylphenol ether-10 are dissolved in 20 parts of deionized water, and then 23.25 parts of methyl methacrylate, 17 parts of butyl acrylate, 4.25 parts of isooctyl acrylate, 1 part of acrylonitrile, 0.25 parts of acrylamide, 1.5 parts of acrylic acid, 0.5 parts of methacrylic acid, 1.25 parts of hydroxyethyl methacrylate and 2 parts of ethoxylated trimethylolpropane triacrylate are added in sequence for emulsification to obtain a shell pre-emulsion;
[0160] A bottom reaction liquid: 0.27 parts of disodium succinate nonylphenol polyoxyethylene ether monoester sulfonate and 0.13 parts of polyoxyethylene octylphenol ether-10 are dissolved in 60 parts of deionized water, and then 0.5 parts of sodium bicarbonate are added to obtain a bottom reaction liquid;
[0161] Initiator solution: Add 0.6 parts of ammonium persulfate to 6 parts of deionized water to obtain an initiator aqueous solution.
[0162] 60.9 parts of the bottom reaction liquid were added to a reactor at 40°C, with a rotation speed of 120rpm. 10.622 parts of the seed emulsion were added to the reactor, heated to 80°C, 0.6 parts of the initiator solution were added, and after reacting for 15 minutes, 64.2 parts of the core pre-emulsion and 2.4 parts of the initiator solution were dripped at the same time. After the dripping was completed, after reacting for 10 minutes, 71.8 parts of the shell pre-emulsion and 3 parts of the initiator solution were dripped into the system at the same time. After the dripping was completed, the reaction was kept at 87°C for 1h. After the reaction was completed, the temperature was lowered to 65°C, 0.05 parts of bleaching powder and 0.048 parts of tert-butyl peroxide were added, and then the temperature was lowered to 35°C. The pH was adjusted to 7.45 using 25% mass percentage concentration of ammonia water, and the material was filtered to obtain the ether-containing core-shell polyacrylic acid water-based adhesive.
[0163] The binders obtained in the examples and comparative examples were subjected to performance tests, and the test methods were as follows:
[0164] (1) Take graphite slurry without adding adhesive, then add an adhesive in an amount of 2% of the solid component of the graphite slurry to the solid component of the adhesive, stir evenly to obtain a mixed slurry. Take 8-10g of the mixed slurry, evenly apply it on the copper foil with a 200um thick applicator, and then bake it in a 75℃ oven for 20 minutes to obtain an electrode. Cut the electrode into 30mm wide strips, use 3M tape to stick the strips to the plywood, use a 2kg standard rolling wheel to roll the strips back and forth 3 times to compact them, and then stretch the strips at a stretching speed of 50mm / min to obtain the peel strength;
[0165] (2) After the adhesive solution is dried at 65°C to form an adhesive film, 1.5 g of the film sample is cut and immersed in an electrolyte at 65°C for 3 days. The swelling ratio is calculated by weighing: swelling ratio = (weight after swelling - weight before swelling) / weight before swelling × 100%;
[0166] The test results are shown in Table 1.
[0167] Table 1
[0168] Peel strength (N / m) Swelling rate (%) Example 1 5.75 63 Example 2 4.95 54 Example 3 6.71 54 Example 4 7.18 58 Example 5 5.67 43 Example 6 5.39 48 Example 7 5.56 57 Example 8 4.79 56 Comparative Example 1 3.83 79 Comparative Example 2 4.15 57 Comparative Example 3 4.56 61
[0169] It can be concluded from the content of Table 1 that the present invention prepares an ether-containing core-shell polyacrylic acid aqueous adhesive that is hard inside and soft outside by designing the monomer types and mass ratios in the core and shell pre-emulsions, and introduces ether bonds, carboxylic acids and carboxylates, and ester groups into the adhesive, so that the prepared core-shell polyacrylic acid aqueous adhesive has better adhesion and lower swelling.
[0170] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the ether-containing core-shell polyacrylic acid water-based adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An ether-containing core-shell polyacrylic acid aqueous adhesive, characterized in that: The ether-containing core-shell polyacrylic acid aqueous adhesive is a polymer with a core-shell structure obtained by polymerizing monomers, wherein the polymerizing monomers include a basic monomer, a first functional monomer, a second functional monomer and a cross-linking monomer; The basic monomer is selected from any one or a combination of at least two of methyl acrylate, methyl methacrylate, ethyl acrylate, styrene, ethyl methacrylate, isopropyl methacrylate, butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, n-octyl acrylate, isooctyl acrylate, lauric acrylate, lauric methacrylate, 2-ethylhexyl acrylate, hexyl methacrylate or vinyl acetate; the first functional monomer is selected from any one or a combination of at least two of acrylic acid, methacrylic acid, acrylonitrile, acrylamide, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, hydroxypropyl methacrylate, 4-hydroxybutyl acrylate; the cross-linking monomer is selected from any one or a combination of at least two of diacetone acrylamide, N-hydroxymethyl acrylamide, divinylbenzene, aziridine, glycidyl methacrylate, ethoxylated trimethylolpropane triacrylate or silane coupling agent.
2. The ether-containing core-shell polyacrylic acid aqueous adhesive according to claim 1, characterized in that: The first functional monomer is selected from any one or a combination of at least two of ethoxyethoxyethyl acrylate, methoxy polyethylene glycol acrylate, polyethylene glycol acrylate or polyethylene glycol diacrylate; Preferably, the polymerized monomers of the core include the following components in parts by weight: 12.5 to 80 parts of basic monomers, 0.25 to 30 parts of second functional monomers, and 0.25 to 15 parts of crosslinking monomers; Preferably, the polymerized monomers of the shell include the following components in percentage by mass: 10 to 75 parts of basic monomers, 0.2 to 30 parts of first functional monomers, 0.2 to 30 parts of second functional monomers and 0.1 to 15 parts of cross-linking monomers.
3. The ether-containing core-shell polyacrylic acid aqueous adhesive according to claim 1 or 2, characterized in that: The ether-containing core-shell polyacrylic acid aqueous adhesive is obtained by emulsion polymerization.
4. The method for preparing the ether-containing core-shell polyacrylic acid aqueous adhesive according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) preparing a core pre-emulsified liquid, a core pre-emulsified seed emulsion, a shell pre-emulsified liquid, a kettle bottom reaction liquid and an initiator solution; (2) adding the pre-emulsified seed emulsion to the reaction liquid at the bottom of the kettle, heating it, adding the initiator solution, and reacting; (3) adding the core pre-emulsion and the initiator solution to the reaction solution obtained in step (2) to react; (4) adding the shell pre-emulsion and the initiator solution to the reaction solution obtained in step (3), reacting to obtain the ether-containing core-shell polyacrylic acid aqueous adhesive.
5. The preparation method according to claim 4, characterized in that: The core pre-emulsion comprises basic monomers, second functional monomers, cross-linking monomers, emulsifiers and deionized water; Preferably, the core pre-emulsion includes 12.25 to 65 parts of basic monomers, 0.245 to 25 parts of second functional monomers and 0.25 to 15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the core pre-emulsion is 0.25% to 4% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the amount of deionized water in the core pre-emulsion is 10%-80% of the total weight of the basic monomer, the second functional monomer and the cross-linking monomer in the core pre-emulsion; Preferably, the core pre-emulsified seed emulsion comprises a basic monomer, a second functional monomer, an emulsifier and deionized water; Preferably, the core pre-emulsified seed emulsion comprises 0.25 to 18 parts of the basic monomer and 0.005 to 8 parts of the second functional monomer; Preferably, the amount of the emulsifier in the core pre-emulsified seed emulsion is 0.005%-1% of the total weight of the basic monomer and the second functional monomer in the core pre-emulsified seed emulsion; Preferably, the amount of deionized water in the core pre-emulsified seed emulsion is 10%-80% of the total weight of the basic monomers, the second functional monomers and the cross-linking monomers in the core pre-emulsified seed emulsion; Preferably, the shell pre-emulsion comprises a basic monomer, a first functional monomer, a second functional monomer, a cross-linking monomer, an emulsifier and deionized water; Preferably, the shell pre-emulsion includes 10 to 75 parts of basic monomers, 0.2 to 30 parts of first functional monomers, 0.2 to 30 parts of second functional monomers and 0.1 to 15 parts of cross-linking monomers; Preferably, the amount of the emulsifier in the shell pre-emulsion is 0.2%-4% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the shell pre-emulsion; Preferably, the amount of deionized water in the shell pre-emulsion is 10%-80% of the total weight of the basic monomer, the first functional monomer, the second functional monomer and the cross-linking monomer in the shell pre-emulsion; Preferably, the reaction liquid at the bottom of the kettle comprises an emulsifier, deionized water and a buffer; Preferably, the contents of the components in the bottom reaction liquid are 0.1 to 3 parts of emulsifier, 50 to 120 parts of deionized water, and 0.25 to 1 part of buffer; Preferably, the emulsifiers in the core pre-emulsified liquid, the core pre-emulsified seed emulsion, the shell pre-emulsified liquid and the bottom reaction liquid are independently selected from any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene octylphenol ether-10, allyloxy fatty alcohol oxyethylene ether ammonium sulfate or disodium succinic acid nonylphenol polyoxyethylene ether monoester sulfonate or a combination of at least two thereof; Preferably, the buffer is sodium bicarbonate, ammonia water, ammonium bicarbonate, or sodium hydroxide; Preferably, the initiator solution comprises an initiator and deionized water; Preferably, the amount of deionized water in the initiator solution is 1 to 20 parts relative to 1 part by weight of the initiator; Preferably, the initiator is selected from inorganic peroxide initiators; Preferably, the initiator is selected from any one or a combination of at least two of potassium persulfate, ammonium persulfate or sodium persulfate; Preferably, the reaction in step (2) to step (4) is carried out under stirring, and the stirring speed is 100-500r / min.
6. The preparation method according to any one of claims 4-5, characterized in that: Before adding the pre-emulsified seed emulsion in step (2), the reaction liquid at the bottom of the kettle is first added into the reaction kettle at 40-75°C; Preferably, the temperature in step (2) is increased to 75-85°C; Preferably, the mass of the reaction liquid at the bottom of the kettle in step (2) is 3 to 85 times that of the seed emulsion pre-emulsified in the core; Preferably, the amount of the initiator solution added in step (2) is 0.06%-15% of the weight of the core pre-emulsified seed emulsion; Preferably, the reaction time in step (2) is 10-30 min; Preferably, the weight ratio of the nuclear pre-emulsion in step (3) to the bottom reaction liquid in step (2) is 1:0.15-1; Preferably, the amount of the initiator solution added in step (3) is 0.0045%-15% of the weight of the core pre-emulsion; Preferably, the reaction temperature in step (3) is 75-85°C; Preferably, the reaction time in step (3) is 10-30 min.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The weight ratio of the core pre-emulsion in step (3) to the shell pre-emulsion in step (4) is 1:0.25-3; Preferably, the amount of the initiator solution added in step (4) is 0.006%-15% of the weight of the shell pre-emulsion; Preferably, the reaction temperature in step (4) is 80-90°C; Preferably, the reaction time in step (4) is 0.5-2.5 h.
8. The preparation method according to any one of claims 4 to 7, characterized in that: After the reaction in step (4) is completed, the temperature is lowered to 60-70° C., a residual monomer eliminator is added, and then the temperature is lowered to below 50° C., the pH is adjusted to 7-8, and the material is filtered to obtain the ether-containing core-shell polyacrylic acid aqueous adhesive; Preferably, the residual monomer eliminator is bleaching powder and tert-butyl peroxide; Preferably, the reagent used to adjust the pH is any one of ammonia water, sodium hydroxide, lithium hydroxide, potassium hydroxide or sodium bicarbonate, or a combination of at least two thereof.
9. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate of the lithium-ion battery comprises the ether-containing core-shell polyacrylic acid aqueous adhesive according to any one of claims 1 to 8.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Adhesive for negative pole material of lithium ion battery and preparation method of electrode containing adhesive
CN103400990A
Anti-fracture pressure sensitive adhesive and preparation method of pressure sensitive adhesive
CN104694054A
Acrylic emulsion resin having excellent adhesive property and preparation method therefor
CN105189580A
Silicon negative electrode adhesive for lithium battery and preparation method of adhesive
CN108929401A
Acrylic emulsion
JP2000001594A
Cited By
Negative electrode binder, negative electrode coating composition, negative electrode pole piece and secondary battery
CN118834636A
A negative electrode binder, a negative electrode coating composition, a negative electrode sheet and a secondary battery
CN118834636B
JPWO2026094859A1
Material for forming nonaqueous secondary battery electrode, binder composition for nonaqueous secondary battery electrode, method for producing material for forming nonaqueous secondary battery electrode, composition for nonaqueous secondary battery electrode, composition for conductive substrate coating, current collector, nonaqueous secondary battery electrode, and nonaqueous secondary battery