High-toughness high-thermal-conductivity die-casting magnesium alloy and preparation method thereof

By designing appropriate Al, La, Ce, Ca and Gd elemental components in magnesium alloys to form a specific second phase structure, the balance problem between strength, toughness and thermal conductivity of magnesium alloy materials is solved, and high strength, high Die-cast magnesium alloy material with thermal conductivity and low cost, suitable for complex structural products.

CN118773498APending Publication Date: 2024-10-15BAOSTEEL METAL CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310772495.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing magnesium alloy materials cannot simultaneously achieve high strength, toughness, high thermal conductivity and low cost, making it difficult to meet the requirements for mechanical properties and thermal conductivity of complex structural products.

Method used

The alloy composition design of elements such as Al, La, Ce, Ca and Gd is used to form second phases such as Al11RE3, Al2RE, Al2Ca, (Mg,Al)2Ca, Al2Gd, etc., the proportion of Al and RE is controlled, and a new phase of needle-shaped Al3RE is introduced. Two phases, optimizing the lattice structure to improve mechanical properties and maintain high thermal conductivity.

Benefits of technology

It has achieved room temperature yield strength of magnesium alloy of 140~150MPa, elongation of 8~12% and thermal conductivity of 100~110W/(m·K). It also reduces process costs and is suitable for 3C products and automotive parts. Thermal dissipation/thermal conduction components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004308332000000161
    Figure BDA0004308332000000161
  • Figure BDA0004308332000000162
    Figure BDA0004308332000000162
  • Figure BDA0004308332000000171
    Figure BDA0004308332000000171
Patent Text Reader

Abstract

The invention discloses a high-toughness and high-thermal-conductivity die-casting magnesium alloy and a preparation method thereof. The high-toughness and high-thermal-conductivity die-casting magnesium alloy comprises the following components in percentage by weight: 2.5-4.0% of Al, 3.5-5.5% of RE, 0.1-0.3% of Mn, 0.002-0.003% of Be, 0.1-1.0% of Ca, 0.05-0.3% of Gd and the balance of Mg and other inevitable impurities, wherein RE is one or two of La and Ce; and the elements also need to simultaneously meet the condition that Al / RE is more than or equal to 0.7 and less than or equal to 0.8. And a new needle-shaped Al3RE second phase is introduced, so that the mechanical property of the material is improved through a more excellent second phase strengthening effect. The negative influence of the Al element on the heat-conducting property of the magnesium alloy is reduced by combining the formation of the second phase, meanwhile, the generation of a brittle phase Mg17Al12 is inhibited, and the remarkable reduction of the heat conductivity is avoided, so that the magnesium alloy with both high heat conductivity and high room-temperature mechanical property is obtained. The room-temperature yield strength of the obtained magnesium alloy is 140-150 MPa, the ductility is 8-12%, and the heat conductivity is 100-110 W / (m.K).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium alloy materials, and in particular to a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy and a preparation method thereof. Background Art

[0002] The cooling system structures of mobile phone mid-plates, laptop computer shells, 5G base station shells, car headlight bases, mobile energy storage devices, etc., not only require their materials to have the characteristics of low density and high strength, but also require them to have excellent thermal conductivity / heat dissipation performance. Magnesium alloy is the metal material with the lowest density in the current engineering structural materials. At the same time, magnesium alloy has excellent thermal conductivity, damping performance and electromagnetic properties, so it is considered to be a very potential structural-functional integrated material. Because magnesium alloy has both lightweight characteristics and excellent physical properties, it has broad application prospects in the above-mentioned 3C products and automotive parts fields.

[0003] The thermal conductivity of pure magnesium at room temperature is about 154.5W / (m·K), but its yield strength is too low to be used as an engineering material. Deformed magnesium alloys have excellent mechanical properties, but conventional extrusion, rolling, and forging of magnesium alloys are expensive, and it is impossible to produce magnesium alloy products with complex structures and shapes. Therefore, more than 80% of magnesium alloy products are formed by die casting. Die casting is the most widely used magnesium alloy casting process. It has the advantages of low manufacturing cost and the ability to form complex structural products. Products such as 3C product housings, 5G base station housings, car headlight bases, mobile energy storage equipment, etc. require their materials to have excellent thermal conductivity / heat dissipation and mechanical properties while being lightweight to ensure that the product has high working stability and service life. In addition, such products usually have complex appearance structures. Considering the cost factor, the die casting process is an ideal choice. The most commonly used die-cast magnesium alloy AZ91D (Mg-9Al-1Zn) is made by adding a certain amount of Al, Zn and other elements to pure magnesium to improve its mechanical properties. However, its thermal conductivity is significantly reduced and its thermal conductivity is only 51.2W / (m·K), which is increasingly unable to meet the demand for magnesium alloy products. Therefore, it is urgent to carry out research on the composition design and forming technology of new magnesium alloys to develop high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy products.

[0004] Chinese patent CN105463280A discloses "a magnesium alloy with high thermal conductivity and its preparation method", and prepares a Mg-Al-RE-Mn die-cast magnesium alloy, whose chemical composition mass percentage is: Al: 3.0-6.8%, Mn: 0.3-0.8%, mixed rare earth (La, Ce, Pr and Nd): 2.8-4.8%, and the rest is Mg. The thermal conductivity of the alloy is greater than 100W / (m·K), but the patent does not mention the mechanical properties of the magnesium alloy.

[0005] Chinese patent CN107604228A discloses "High thermal conductivity and corrosion resistant die-cast magnesium alloy and its preparation method", and prepares Mg-Al-Ce-Mn-Be die-cast magnesium alloy, whose chemical composition mass percentage is: Ce: 3.5-5.0%, Al: 2.5-3.5%, Mn: 0.5%, Be: 0.05%, and the rest is Mg. The thermal conductivity of the alloy is greater than 100W / (m·K), and the tensile strength is 250-260MPa, but key mechanical properties such as yield strength and elongation of magnesium alloy are not mentioned.

[0006] Chinese patent CN114351022A discloses "a high thermal conductivity magnesium alloy containing high solid solubility rare earth elements and its preparation method", and prepares a Mg-RE-Al casting magnesium alloy, whose chemical composition is: RE: 4-16% (mass percentage), Al: the atomic ratio of Al to RE is 0.3-4%, and the rest is Mg. The thermal conductivity of the alloy is ≥100W / (m·K), but the alloy contains a large amount of precious rare earth element Sm, the cost is high, and the mechanical properties are not mentioned.

[0007] The die-cast magnesium alloy materials reported in the prior art cannot simultaneously take into account high strength, toughness, high thermal conductivity and processing cost. Therefore, it is urgently necessary to carry out new die-cast magnesium alloy composition design and new molding technology research to develop new high-strength, toughness and high-thermal conductivity die-cast magnesium alloys to expand the application of magnesium alloys. Summary of the invention

[0008] The purpose of the present invention is to provide a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy and a preparation method thereof. Without adding expensive rare earth elements or other alloy elements, a low-cost alloy composition design is adopted to ensure that the alloy has good casting performance, thereby solving the problem that the existing magnesium alloy cannot simultaneously take into account high mechanical properties and high thermal conductivity. The room temperature thermal conductivity of the magnesium alloy is 100-110 W / (m·K), the room temperature yield strength is 140-150 MPa, and the room temperature elongation is 8-12%. The process cost is low, and it is convenient for large-scale mass production, and can be widely used in the manufacture of magnesium alloy products with complex structures, such as 3C products and heat dissipation / thermal conductive components in the field of automotive parts.

[0009] To achieve the above object, the technical solution of the present invention is:

[0010] A high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy, the composition weight percentage of which is: Al: 2.5-4.0%, RE: 3.5-5.5%, Mn: 0.1-0.3%, Be: 0.002-0.003%, Ca: 0.1-1.0%, Gd: 0.05-0.3%, RE is one or both of La or Ce, and the balance includes Mg and other inevitable impurities; and the above elements also need to meet the following requirements at the same time:

[0011] 0.7≤Al / RE≤0.8.

[0012] Preferably, the balance is Mg and other inevitable impurities.

[0013] The die-cast magnesium alloy matrix of the present invention is uniformly distributed with Al 11 RE3, Al2RE, Al2Ca, (Mg,Al)2Ca, Al2Gd and needle-shaped Al3RE second phase.

[0014] The room temperature yield strength of the die-cast magnesium alloy of the present invention is 140-150 MPa, the elongation is 8-12%, and the thermal conductivity is 100-110 W / (m·K).

[0015] Al is the most commonly used alloying element in magnesium alloys, and Mg-Al alloys have good casting properties. However, the atomic volume of Al is smaller than that of Mg. As Al atoms dissolve in Mg, the lattice volume gradually decreases. The smaller the lattice volume, the greater the possibility of free electron scattering, and the more obvious the negative effect on thermal conductivity. In addition, the valence electron difference between Al atoms and Mg atoms also leads to a significant reduction in the thermal conductivity of magnesium alloys when Al is dissolved in Mg. For example, the thermal conductivity of the commercial die-cast magnesium alloy AZ91D is only 51.2W / (m·K).

[0016] In the present invention, elements such as La, Ce, Ca and Gd having strong affinity with Al are added to form Al 11 RE3, Al2RE, Al2Ca, (Mg,Al)2Ca, Al2Gd second phases, and introduced a new needle-shaped Al3RE second phase. This needle-shaped second phase is stronger than Al 11 The second phase of RE3 is smaller in size and has a more excellent second phase strengthening effect, which significantly improves the mechanical properties of the material. These second phases not only improve the mechanical properties of the material, but also consume the Al element in the Mg matrix, increase the lattice volume, reduce the possibility of free electron scattering, and avoid the decrease in the thermal conductivity of the material caused by the solid solution of the Al element in the magnesium alloy. As a result, the magnesium alloy has both high mechanical properties and high thermal conductivity.

[0017] In Mg-Al alloys, when the Al content is less than 2.5%, the die casting performance is affected and the fluidity of the magnesium melt is poor; when the Al content is higher than 4%, the thermal conductivity is significantly reduced. Therefore, in the present invention, the Al content is controlled at 2.5-4%.

[0018] La and Ce form a large amount of Al 11 RE3 second phase and a small amount of Al2RE second phase, wherein the added Al and RE elements are controlled to satisfy 0.7≤Al / RE≤0.8, so that Al and RE are in the form of fine lamellar Al 11RE3, extremely fine needle-like Al3RE second phase and granular Al2RE second phase exist in the original Al 11 On the basis of the existence of RE3 and Al2RE second phases, the introduction of a new second phase Al3RE has a more excellent second phase strengthening effect and significantly improves the mechanical properties of the material. 11 The formation of the second phases of RE3, Al3RE and Al2RE largely avoids the existence of Al in the form of solid solution atoms in the magnesium alloy, reduces the negative impact of the Al element on the thermal conductivity of the magnesium alloy, and thus does not lead to a decrease in the thermal conductivity of the material, ensuring that the magnesium alloy has both excellent thermal conductivity and mechanical properties. The cheap rare earth elements La and Ce also have the function of purifying the magnesium alloy melt. Too little La and Ce elements cannot form enough Al-RE second phases to improve material properties. When La and Ce are added in excess of 5.5%, the die-casting performance of the magnesium alloy is significantly reduced, and the melt fluidity deteriorates. Too much RE will also increase the material cost. Therefore, in the present invention, the amount of RE (La and Ce) is controlled at 3.5-5.5%.

[0019] The fine dispersed Al2Ca second phase and (Mg,Al)2Ca second phase formed by the Ca element and Al in the Mg-Al alloy can significantly improve the room temperature mechanical properties of the magnesium alloy, while ensuring that the material has excellent plasticity and toughness. In addition, the presence of the second phase Al2Ca in the magnesium alloy does not significantly reduce the thermal conductivity of the material. In addition, Ca also has the effect of anti-oxidation and flame retardancy in the magnesium alloy, inhibits the oxidation of the surface of the magnesium alloy melt during die casting, and greatly reduces the inclusions in the die-cast magnesium alloy. However, too much Ca element will reduce the fluidity of the magnesium solution during die casting, increase the tendency to hot cracking and brittleness, and reduce the mechanical properties of the material. Therefore, in the present invention, the Ca element content is controlled at 0.1-1%.

[0020] The solid solubility of Mn element in magnesium alloy is extremely low, which can effectively reduce the content of harmful elements such as Fe, Cu, Ni in magnesium alloy to improve the corrosion resistance of magnesium alloy. In addition, an appropriate amount of Mn has the effect of refining the cast structure of magnesium alloy, which can improve the plasticity and toughness of the material and has a small negative impact on thermal conductivity. However, adding more than 0.3% of Mn in the present invention will reduce the effect of grain refinement. Therefore, the content of Mn element is controlled to 0.1-0.3% in the present invention.

[0021] The affinity of Be to oxygen is greater than that of Mg to oxygen. A very small amount of Be can form a dense oxide film on the surface of the magnesium alloy melt to prevent the magnesium alloy melt from oxidation. When the Be content is lower than 0.002%, the degree of oxidation of the magnesium alloy solution is significantly increased. When the Be content is higher than 0.003%, the microstructure of the material is significantly coarsened and the mechanical properties are reduced. Therefore, in the present invention, the Be content is controlled at 0.002-0.003%, the slag and inclusions in the magnesium alloy solution are reduced, the mechanical properties of the material are improved, and the inclusions and oxides are prevented from reducing the thermal conductivity of the material.

[0022] When Gd is added to Mg-Al alloy, a large amount of network Mg is precipitated at the grain boundary of conventional Mg-Al alloy during solidification. 17 Al 12 The second phase distributed at the grain boundary seriously destroys the periodic arrangement of the magnesium matrix lattice and scatters the free electrons, thereby reducing the thermal conductivity of the material. The addition of Gd element in the present invention can form Al2Gd second phase with Al element, thereby inhibiting the brittle phase Mg 17 Al 12 The formation of Gd can avoid a significant decrease in thermal conductivity. The Al2Gd phase formed at the same time has a significant strengthening effect, which improves the strength of the magnesium alloy without significantly reducing the plasticity of the material. In addition, the Al2Gd phase can also promote the heterogeneous nucleation process, increase the nucleation rate during die casting solidification, and refine the grain size and microstructure. Too little Gd element cannot play a strengthening effect and inhibit Mg in magnesium alloys. 17 Al 12 Too much Gd addition will reduce the die-casting performance of the magnesium alloy. Therefore, in the present invention, the Gd content is controlled within the range of 0.05-0.3%.

[0023] Therefore, the present invention obtains a die-cast magnesium alloy having both high strength and high toughness by controlling the composition while ensuring that the magnesium alloy has excellent casting properties.

[0024] The method for preparing the high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy of the present invention comprises the following steps:

[0025] 1) Ingredients

[0026] Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder and Mg-Ca, Mg-Gd, Al-Be master alloys as raw materials, the ingredients are prepared according to the above magnesium alloy composition;

[0027] 2) Melting

[0028] Putting a pure Mg ingot into a crucible, heating it to 680-710°C, and completely melting it under the protection of a protective gas, then adding a pure Al ingot and a pure Mn powder, stirring it under the protective atmosphere until the alloy is completely melted, then heating it to 740-750°C, and then sequentially adding a pure La ingot and a pure Ce ingot, stirring it under the protective atmosphere until the alloy is completely melted, then cooling it to 690-710°C, adding Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, and stirring it for 5-10 minutes after the master alloy is completely melted, to obtain a magnesium alloy melt;

[0029] 3) Refining

[0030] Adding magnesium alloy flux to the obtained magnesium alloy melt, refining for 5 to 10 minutes, removing surface scum, and then heating to 700 to 720° C. and keeping the temperature for 10 to 15 minutes;

[0031] 4) Molding

[0032] The refined magnesium alloy melt is cast into an ingot, which is then placed in a die-casting machine furnace to melt at 680-700°C. The melt enters the mold through an injection system for filling, wherein the mold temperature is 200-250°C, the casting pressure is 100-110 MPa, and the injection speed is 3-5 m / s.

[0033] Preferably, in step 3), the magnesium alloy flux is RJ-2 flux and RJ-3 flux.

[0034] Preferably, in step 2), the protective gas is a mixed gas of CO2+SF6.

[0035] Preferably, in step 4), the pouring temperature is 680-700°C.

[0036] In the die-casting process of the present invention, the furnace temperature is controlled at 680-700°C, while ensuring that the magnesium alloy solution has good fluidity and filling properties, coarse dendrites in the material are avoided to affect the mechanical properties of the material. When the temperature is lower than 680°C, the fluidity of the magnesium alloy solution deteriorates and defects appear on the surface of the filled product. When the temperature is higher than 700°C, coarse dendrites appear in the microstructure of the filled product and the mechanical properties of the material are reduced.

[0037] The mold temperature is controlled at 200-250℃. Within this temperature range, the alloy is fully filled, defects such as cracks and pores are greatly reduced, and the material has excellent mechanical properties. When the temperature is lower than 200℃, due to the large temperature difference between the high-temperature melt and the mold temperature, defects appear on the surface of the filled product, and the plasticity of the product is reduced; when the mold temperature is higher than 250℃, the fine grain area on the product surface is reduced, and the mechanical properties are reduced.

[0038] The casting pressure is 100-110MPa to ensure normal filling of the product, making the material's microstructure dense, and having excellent mechanical properties and thermal conductivity.

[0039] The injection speed is controlled at 3-5m / s. If the injection speed is too low, the material cannot be completely filled into the mold. If the injection speed is too high, the material porosity is high, and the mechanical properties and thermal conductivity will be reduced.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The high-strength, high-toughness and high-thermal-conductivity magnesium alloy of the present invention adds Al, La, Ce, Ca and Gd elements to the magnesium matrix to form Al 11 RE3, Al2RE, Al2Ca, (Mg,Al)2Ca, Al2Gd second phases. At the same time, the added Al and RE elements are controlled to meet 0.7≤Al / RE≤0.8, and a needle-shaped Al3RE new second phase is introduced to improve the mechanical properties of the material with a more excellent second phase strengthening effect; and the formation of these second phases greatly avoids the existence of Al in the form of solid solution atoms in the magnesium alloy, reducing the negative impact of Al on the thermal conductivity of the magnesium alloy, thereby not causing a decrease in the thermal conductivity of the material. Combined with the addition of Gd elements and Al elements to form Al2Gd second phases, the brittle phase Mg 17 Al 12 The formation of magnesium alloys avoids a significant decrease in thermal conductivity, thereby obtaining a magnesium alloy with both high thermal conductivity and high room temperature mechanical properties.

[0042] The alloy elements added in the present invention ensure the material properties while taking into account the die-casting manufacturability. Based on the composition design, the appropriate furnace temperature, mold temperature, casting pressure and injection speed are matched at the same time, so that the magnesium alloy has good fluidity and filling properties during die-casting, the product microstructure is dense and defect-free, the process cost is low, and complex structural products such as 3C housings, automotive parts, etc. with complex appearance structures can be mass-produced.

[0043] The room temperature thermal conductivity of the magnesium alloy obtained by the invention is 100-110 W / (m·K), the room temperature yield strength is 140-150 MPa, and the room temperature elongation is 8-12%. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is described in detail below through examples. This example is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following examples.

[0045] The magnesium alloy composition of the embodiment of the present invention is shown in Table 1, and the rest is Mg and other inevitable impurities.

[0046] Example 1

[0047] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0048] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0049] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 700°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir it under the protective atmosphere until the alloy is completely melted, then heat it to 740°C, and then sequentially add the pure La ingot and the pure Ce ingot under the protective atmosphere, stir it until the alloy is completely melted, let it stand and cool to 710°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir it for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 for refining for 10 minutes, remove the surface scum, and finally keep it at 700°C for 15 minutes to cast it into a magnesium alloy ingot;

[0050] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 680°C. The melt enters the mold through the injection system for filling. The mold temperature is 216°C, the casting pressure is 105MPa, and the injection speed is 3.5m / s.

[0051] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0052] Example 2

[0053] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0054] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0055] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 690°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 741°C, and then sequentially add the pure La ingot and the pure Ce ingot under the protective atmosphere, stir until the alloy is completely melted, let it stand and cool to 700°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 6 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-3 and refine for 7 minutes, remove the surface scum, and finally keep it at 710°C for 12 minutes to cast it into a magnesium alloy ingot;

[0056] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 692°C. The melt enters the mold through the injection system for filling, wherein the mold temperature is 220°C, the casting pressure is 100 MPa, and the injection speed is 3 m / s.

[0057] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0058] Example 3

[0059] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0060] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0061] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 710°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 750°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 705°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 10 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 10 minutes, remove the surface scum, and finally keep it at 705°C for 11 minutes to cast it into a magnesium alloy ingot;

[0062] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 700°C. The melt enters the mold through the injection system for filling. The mold temperature is 239°C, the casting pressure is 101MPa, and the injection speed is 4m / s.

[0063] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0064] Example 4

[0065] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0066] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0067] 2) Put the pure Mg ingot into the crucible of the melting furnace, heat it to 695°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 749°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 708°C, add Al-Be, Mg-Ca and Mg-Gd intermediate alloys into the melt, stir for 10 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-3 and refine for 9 minutes, remove the surface scum, and finally keep it at 710°C for 15 minutes to cast it into a magnesium alloy ingot;

[0068] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 695°C. The melt enters the mold through the injection system for filling. The mold temperature is 250°C, the casting pressure is 110MPa, and the injection speed is 3.3m / s.

[0069] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0070] Example 5

[0071] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0072] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0073] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 705°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 748°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 706°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 10 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 10 minutes, remove the surface scum, and finally keep it at 720°C for 10 minutes to cast it into a magnesium alloy ingot;

[0074] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 688°C. The melt enters the mold through the injection system for filling. The mold temperature is 208°C, the casting pressure is 108MPa, and the injection speed is 4.3m / s.

[0075] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0076] Example 6

[0077] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0078] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0079] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 680°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 745°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 690°C, add Al-Be, Mg-Ca and Mg-Gd intermediate alloys into the melt, stir for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 5 minutes, remove the surface scum, and finally keep it at 705°C for 11 minutes to cast it into a magnesium alloy ingot;

[0080] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 690°C. The melt enters the mold through the injection system for filling, wherein the mold temperature is 200°C, the casting pressure is 109 MPa, and the injection speed is 5 m / s.

[0081] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0082] Example 7

[0083] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0084] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0085] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 700°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 743°C, and then sequentially add the pure La ingot and the pure Ce ingot under the protective atmosphere, stir until the alloy is completely melted, let it stand and cool to 695°C, add Al-Be, Mg-Ca and Mg-Gd intermediate alloys into the melt, stir for 8 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 for refining for 8 minutes, remove the surface scum, and finally keep it at 713°C for 11 minutes to cast it into a magnesium alloy ingot;

[0086] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 695°C. The melt enters the mold through the injection system for filling. The mold temperature is 226°C, the casting pressure is 102MPa, and the injection speed is 4.6m / s.

[0087] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0088] Example 8

[0089] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0090] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0091] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 690°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 744°C, and then sequentially add the pure La ingot and the pure Ce ingot under the protective atmosphere, stir until the alloy is completely melted, let it stand and cool to 705°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 7 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 and refine for 7 minutes, remove the surface scum, and finally keep it at 720°C for 15 minutes to cast it into a magnesium alloy ingot;

[0092] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 698°C. The melt enters the mold through the injection system for filling. The mold temperature is 239°C, the casting pressure is 103MPa, and the injection speed is 3.1m / s.

[0093] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0094] Example 9

[0095] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0096] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0097] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 710°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 746°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 694°C, add Al-Be, Mg-Ca and Mg-Gd intermediate alloys into the melt, stir for 7 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 and refine for 6 minutes, remove the surface scum, and finally keep it at 715°C for 11 minutes to cast it into a magnesium alloy ingot;

[0098] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 685°C. The melt enters the mold through the injection system for filling. The mold temperature is 203°C, the casting pressure is 104MPa, and the injection speed is 3.9m / s.

[0099] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0100] Example 10

[0101] A method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy comprises the following steps:

[0102] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0103] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 705°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 747°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 698°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 5 minutes, remove the surface scum, and finally keep it at 718°C for 15 minutes to cast it into a magnesium alloy ingot;

[0104] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 689°C. The melt enters the mold through the injection system for filling. The mold temperature is 245°C, the casting pressure is 106MPa, and the injection speed is 4.8m / s.

[0105] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0106] Comparative Examples 1 and 2 respectively use commercial grades AZ91D and AM60, and the molding process of these two grades of alloys is the traditional die-casting process. The present invention adopts the design principle of high-strength, toughness and high-thermal conductivity magnesium alloy, and the molding process is the die-casting molding process.

[0107] Comparative Example 1

[0108] A method for preparing a die-cast magnesium alloy, wherein the percentage of the magnesium alloy components is selected as follows: 9wt% Al, 1wt% Zn, and the rest is Mg;

[0109] A pure Mg ingot is placed in a crucible of a smelting furnace, heated to 695°C, and completely melted to form a melt under the protection of a mixed protective gas of CO2 and SF6. Subsequently, a pure Al ingot and a pure Zn ingot are added, and stirred for 8 minutes in the mixed protective atmosphere. After the alloy is completely melted, a magnesium alloy flux RJ-2 is added and refined for 7 minutes to remove surface scum. Finally, the alloy is kept at 720°C for 15 minutes and cast into a magnesium alloy ingot. The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 680°C. The melt enters the mold for filling through the injection system, wherein the mold temperature is 206°C, the casting pressure is 105MPa, and the injection speed is 3.5m / s.

[0110] Comparative Example 2

[0111] A method for preparing a die-cast magnesium alloy, wherein the percentage of the components of the magnesium alloy is selected as follows: 6wt% Al, 0.5wt% Mn, and the rest is Mg;

[0112] A pure Mg ingot is placed in a crucible of a smelting furnace, heated to 710°C, and completely melted to form a melt under the protection of a mixed protective gas of CO2 and SF6. Subsequently, a pure Al ingot and pure Mn powder are added, and stirred for 10 minutes in the mixed protective atmosphere. After the alloy is completely melted, a magnesium alloy flux RJ-2 is added and refined for 10 minutes to remove surface scum. Finally, the alloy is kept at 720°C for 10 minutes and cast into a magnesium alloy ingot. The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 700°C. The melt enters the mold through the injection system for filling, wherein the mold temperature is 209°C, the casting pressure is 105MPa, and the injection speed is 3.9m / s.

[0113] Comparative Example 3

[0114] A method for preparing a die-cast magnesium alloy comprises the following steps:

[0115] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0116] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 703°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 747°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 695°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 5 minutes, remove the surface scum, and finally keep it at 718°C for 15 minutes to cast it into a magnesium alloy ingot;

[0117] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 695°C. The melt enters the mold through the injection system for filling, wherein the mold temperature is 220°C, the casting pressure is 100 MPa, and the injection speed is 3.5 m / s.

[0118] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0119] Comparative Example 4

[0120] A method for preparing a die-cast magnesium alloy comprises the following steps:

[0121] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be, Mg-Ca and Mg-Gd master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0122] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 705°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 740°C, and then sequentially add the pure La ingot and the pure Ce ingot in the protective atmosphere, stir until the alloy is completely melted, let it stand and cool to 700°C, add Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, stir for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 5 minutes, remove the surface scum, and finally keep it at 718°C for 15 minutes to cast it into a magnesium alloy ingot;

[0123] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 700°C. The melt enters the mold through the injection system for filling. The mold temperature is 230°C, the casting pressure is 103MPa, and the injection speed is 3m / s.

[0124] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0125] Comparative Example 5

[0126] A method for preparing a die-cast magnesium alloy comprises the following steps:

[0127] 1) Using pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder, and Al-Be and Mg-Ca master alloys as raw materials, the ingredients are prepared according to the weight percentage of the magnesium alloy components designed;

[0128] 2) Put the pure Mg ingot into the crucible of the smelting furnace, heat it to 709°C, and completely melt it under the protection of the mixed protective gas of CO2 and SF6 to form a melt, then add the pure Al ingot and pure Mn powder, stir until the alloy is completely melted under the protective atmosphere, then heat it to 739°C, and then sequentially add the pure La ingot and the pure Ce ingot, stir until the alloy is completely melted under the protective atmosphere, let it stand and cool to 698°C, add Al-Be and Mg-Ca master alloys to the melt, stir for 5 minutes after the alloy is completely melted, then add the magnesium alloy flux RJ-2 to refine for 5 minutes, remove the surface scum, and finally keep it at 718°C for 15 minutes to cast it into a magnesium alloy ingot;

[0129] 3) The magnesium alloy ingot is placed in a 650T die-casting machine furnace and melted at 710°C. The melt enters the mold through the injection system for filling. The mold temperature is 215°C, the casting pressure is 101MPa, and the injection speed is 3.6m / s.

[0130] The properties of the obtained die-cast magnesium alloy parts are shown in Table 3.

[0131] Combined with the data in Table 3, it can be seen that the room temperature thermal conductivity of the magnesium alloy of the present invention is 100-110 W / (m·K), the room temperature yield strength is 140-150 MPa, and the room temperature elongation is 8-12%. The magnesium alloy obtained by the present invention has significantly improved room temperature mechanical properties and thermal conductivity compared with traditional AZ91D magnesium alloy and AM60B magnesium alloy.

[0132] The traditional die-cast AZ91D magnesium alloy and die-cast AM60B magnesium alloy use Al as the main alloying element, which plays a role in solid solution strengthening and the second phase (Mg 17 Al 12) strengthening effect to improve the room temperature yield strength of the material, and adding a small amount of Zn and Mn to further improve the comprehensive mechanical properties of the material; however, this strengthening effect is limited, and at the same time, when more Al elements are dissolved in the magnesium matrix, the thermal conductivity of the material is significantly reduced.

[0133] It can be seen from the comparative examples in Table 3 that the thermal conductivity of the die-cast AZ91D magnesium alloy in comparative example 1 and the die-cast AM60B magnesium alloy in comparative example 2 are both less than 65 W / (m·K), the room temperature yield strength is less than 150 MPa, and the elongation is less than 10%, that is, they cannot have both excellent mechanical properties and thermal conductivity.

[0134] In Comparative Example 3, the Al content and RE content are low, and the second phase strengthening effect is weak, so the material yield strength is only 131 MPa, the elongation is 10%, and the thermal conductivity is 95 W / (m·K).

[0135] In Comparative Example 4, the Al / RE mass ratio is 1, and more Al elements are dissolved in the Mg matrix or form more Mg 17 Al 12 Phase, alloy elements have a more obvious negative effect on thermal conductivity, so the material yield strength is 138MPa, elongation is 11%, and thermal conductivity is 90W / (m·K).

[0136] In Comparative Example 5, no Gd element was added, and Al element formed more Mg at the grain boundary. 17 Al 12 phase, so the material has a yield strength of 139 MPa, an elongation of 10.6%, and a thermal conductivity of 91 W / (m·K).

[0137] Table 1 Unit: Weight percentage

[0138]

[0139] Table 2

[0140]

[0141]

[0142] Table 3

[0143]

[0144]

Claims

1. A high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy, the composition weight percentage of which is: Al: 2.5-4.0%, RE: 3.5-5.5%, Mn: 0.1-0.3%, Be: 0.002-0.003%, Ca: 0.1-1.0%, Gd: 0.05-0.3%, RE is one or both of La or Ce, and the balance includes Mg and other inevitable impurities; and the above elements also need to meet the following requirements at the same time: 0.7≤Al / RE≤0.

8.

2. The high-strength, toughness and high-thermal-conductivity die-cast magnesium alloy according to claim 1, characterized in that: The balance is Mg and other inevitable impurities.

3. The high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy according to claim 1 or 2, characterized in that: The die-cast magnesium alloy matrix is ​​uniformly distributed with Al 11 RE3, Al2RE, Al2Ca, (Mg,Al)2Ca, Al2Gd and needle-shaped Al3RE second phase.

4. The high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy according to claim 1, 2 or 3, characterized in that: The room temperature yield strength of the die-cast magnesium alloy is 140-150 MPa, the elongation is 8-12%, and the thermal conductivity is 100-110 W / (m·K).

5. The method for preparing a high-strength, high-toughness and high-thermal-conductivity die-cast magnesium alloy according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) Ingredients Pure Mg ingots, pure Al ingots, pure La ingots, pure Ce ingots, pure Mn powder and Mg-Ca, Mg-Gd, Al-Be master alloys are used as raw materials and the magnesium alloy composition according to claim 1 or 2 is prepared; 2) Melting Putting a pure Mg ingot into a crucible, heating it to 680-710°C, and completely melting it under the protection of a protective gas, then adding a pure Al ingot and a pure Mn powder, stirring it under the protective atmosphere until the alloy is completely melted, then heating it to 740-750°C, and then sequentially adding a pure La ingot and a pure Ce ingot, stirring it under the protective atmosphere until the alloy is completely melted, then cooling it to 690-710°C, adding Al-Be, Mg-Ca and Mg-Gd master alloys into the melt, and stirring it for 5-10 minutes after the master alloy is completely melted, to obtain a magnesium alloy melt; 3) Refining Adding magnesium alloy flux to the obtained magnesium alloy melt, refining for 5 to 10 minutes, removing surface scum, and then heating to 700 to 720° C. and keeping the temperature for 10 to 15 minutes; 4) Die casting The refined magnesium alloy melt is cast into an ingot, which is then placed in a die-casting machine furnace to melt at 680-700°C. The melt enters the mold through an injection system for filling, wherein the mold temperature is 200-250°C, the casting pressure is 100-110 MPa, and the injection speed is 3-5 m / s.

6. The preparation method according to claim 5, characterized in that: In step 3), the magnesium alloy flux is RJ-2 flux and RJ-3 flux.

7. The preparation method according to claim 5, characterized in that: In step 2), the protective gas is a mixed gas of CO2+SF6.

8. The preparation method according to claim 5, characterized in that: In step 4), the pouring temperature is 680-700°C.

Citation Information

Cited By

  • Magnesium alloy material, preparation method thereof and vehicle structural part

    CN121183188A

  • A magnesium alloy material and its preparation method, and a vehicle structural component.

    CN121183188B