High-damping zirconium-based amorphous composite material and preparation method thereof

By introducing alloying elements and interstitial elements into the Zr-based alloy, the second phase of the body-centered cubic structure is formed and coupled with the amorphous matrix, and a zirconium-based amorphous composite material with high damping performance is developed, solving the research on the damping performance of amorphous alloy materials. It solves the problems of blank and impurity sensitivity and achieves high strength, corrosion resistance and expanded application fields.

CN118773523AActive Publication Date: 2024-10-15DALIAN UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410792952.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-15
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

The existing technology has not yet developed a study on the damping performance of amorphous alloy materials based on the Snoek relaxation mechanism, and amorphous alloys are sensitive to impurity elements, resulting in limited applications.

Method used

Using a Zr-based alloy with both high oxygen solid solubility and high amorphous formation ability as the matrix, through composition and structure control, a body-centered cubic structure second phase is formed to couple with the amorphous matrix, inducing the Snoek relaxation mechanism, and developing a high-performance Damping properties of zirconium-based amorphous composites.

Benefits of technology

It achieves the high damping performance of amorphous matrix composite materials, while maintaining the high strength and high corrosion resistance of amorphous alloys, expanding its application fields and scope, and improving room temperature plastic deformation capacity and fracture strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773523A_ABST
    Figure CN118773523A_ABST
Patent Text Reader

Abstract

The invention discloses a high-damping zirconium-based amorphous composite material and a preparation method thereof, belongs to the field of functional material research, development and preparation, and relates to a Snoek type high-damping zirconium-based amorphous composite material containing a second phase of a body-centered cubic structure, the general formula of atomic percent components of the Snoek type high-damping zirconium-based amorphous composite material is (Zr63.5-aMaAl9Cu23Fe4.5) 100-bXb, M is Nb, Ti or Hf, and X is O, C or B, 0.5 < = a < = 4.5, 0.1 < = b < = 0.5. In the preparation process, industrial pure Zr, M, Fe, Al, Cu and N are used as raw materials, a vacuum arc melting technology is used for melting an alloy ingot, the required alloy material is obtained through a copper mold casting technology, and the damping performance Q-1 value of the alloy material is 0.011-0.015. The amorphous matrix composite material has high damping performance while maintaining the performance advantages of the amorphous matrix composite material, and the application field and range of amorphous materials are expanded; the material has more excellent room-temperature plastic deformation capacity and breaking strength; the Snoek relaxation peak temperature in the material is lower than the glass transition temperature of an amorphous matrix, the material is used at the optimal damping temperature, and the alloy has excellent structure stability and is not prone to glass transition or crystallization instability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-damping zirconium-based amorphous composite material and a preparation method thereof, and belongs to the field of research and development and preparation of metallic functional materials. Background Art

[0002] Damping alloys are a type of functional alloy that relies on its own structure or physical properties to consume energy under cyclic loads to achieve vibration reduction. Using damping alloys in mechanical equipment can effectively solve vibration problems and improve the accuracy, service stability and safety of mechanical parts.

[0003] Recently, a new type of damping alloy with a body-centered cubic structure has been discovered. Small atoms such as O, C, and B in the interstitial position can reciprocate under load and consume energy (i.e., Snoek relaxation mechanism) to achieve vibration reduction. Since the reciprocating motion of small atoms hardly damages the alloy matrix, the damping alloy based on the Snoek relaxation mechanism has a very long service life.

[0004] Amorphous alloys are special alloys with short-range order and long-range disorder in their structure. Compared with crystalline alloys, they often have better mechanical, physical and chemical properties, and have shown broad application prospects in the fields of machinery, medicine, chemical industry and aviation.

[0005] However, there has been no research on the damping properties of amorphous alloy materials based on the Snoek relaxation mechanism. We noticed that there are a large number of tetrahedral and octahedral interstitial positions in the amorphous short-range structure and the structure of its corresponding crystallized phase, which can be used for the solid solution and migration of small atoms such as O, C, and B, providing the possibility of carrying the Snoek relaxation mechanism. Therefore, we combined the high strength and high corrosion resistance of amorphous materials themselves, and developed alloys with high damping properties based on amorphous materials, which will further broaden the application field and scope of amorphous alloy materials.

[0006] Since amorphous alloys are extremely sensitive to impurity elements (such as O), the presence of impurity elements will generally drastically reduce the alloy's amorphous forming ability. Therefore, people will strictly control the purity of the alloy raw materials and the preparation conditions to avoid their introduction. The applicant of this patent uses a Zr-based alloy with both high oxygen solubility and high amorphous forming ability as the matrix, and through the regulation of composition and organization, it makes its endogenous dispersed body-centered cubic structure second phase form an amorphous-based composite material, and at the same time intentionally dissolves a certain amount of small atoms such as O, C, and B into the composite material. On this basis, the effect of coupling the body-centered cubic structure second phase with the amorphous matrix to induce the Snoek relaxation mechanism is achieved, achieving a high damping (Q -1 >0.01) performance. This provides a new idea and approach for the development and application of amorphous composite materials in the damping field. Summary of the invention

[0007] The purpose of the present invention is to broaden the application field and scope of amorphous materials, develop new zirconium-based amorphous composite materials with high damping performance, and provide a candidate system for high-strength and toughness damping alloy materials.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A high damping zirconium-based amorphous composite material, specifically a Snoek-type high damping zirconium-based amorphous composite material containing a body-centered cubic structure second phase. The constituent elements include Zr, M, Fe, Al, Cu, and X. The atomic percentage composition formula of the material is: (Zr 63.5-a M a Al9Cu 23 Fe 4.5 ) 100-b X b , M=Nb, Ti or Hf, X=O, C or B, where 0.5≤a≤4.5, 0.1≤b≤0.5; The damping performance Q of high damping amorphous composite material -1 The value is 0.011~0.015.

[0010] A method for preparing a high-damping zirconium-based amorphous composite material, wherein the preparation method uses commercial industrial pure Zr, M, Fe, Al, Cu, and N as raw materials (wherein M is Nb, Ti, or Hf, and N is C, B, or ZrO2, wherein ZrO2 provides O in the composition elements), wherein the atomic percentage composition is (Zr 63.5-a M a Al9Cu 23 Fe 4.5 ) 100-b X b The target alloy is first melted by vacuum arc melting technology to form alloy ingots, and then the required alloy material plates are obtained by copper mold casting technology. The specific process includes the following steps:

[0011] Step 1: Melting of alloy ingots

[0012] Commercial industrial pure Zr, M, Fe, Al, Cu, N are used as raw materials to prepare the atomic percentage composition (Zr 63.5- a M a Al9Cu 23 Fe 4.5 ) 100-b X bThe target alloy is prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, then evacuating to 1-10 Pa, and filling with 0.01-0.10 MPa industrial pure argon gas for melting; the arc melting working current is 260-290 A, and the melting is repeated for many times to obtain a target alloy ingot with uniform composition. The mass loss rate of the alloy ingot before and after melting is controlled within 10 / 1000.

[0013] Step 2: Suction casting of alloy sheet

[0014] The target alloy ingot obtained in step 1 is placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 1-10Pa, filled with 0.01-0.10MPa of industrial pure argon as a protective gas, and arc melting and copper mold suction casting technology are used. Under an arc with a working current of 360-380A, the target alloy ingot is melted and sucked into a water-cooled copper mold chamber, the mold is cooled to room temperature, and a plate-shaped sample is obtained. The phase composition, organizational morphology, thermal properties and internal friction properties of the sample are characterized and tested at room temperature using an X-ray diffractometer, a scanning electron microscope, a thermal analyzer and a dynamic mechanical analyzer.

[0015] The principle of the present invention is:

[0016] Low-cost Zr with high amorphous forming ability 63.5 Al9Cu 23 Fe 4.5 Alloy is used as the basis, alloying elements Ti, Nb or Hf and interstitial elements O, C or B are introduced into the alloy, and the organization is regulated to make the body-centered cubic structure second phase endogenously dispersed in the amorphous alloy to form an amorphous-based composite material, so as to achieve the effect of the coupling of the body-centered cubic structure second phase and the amorphous matrix to trigger the Snoek relaxation mechanism, so that the alloy has high damping performance while also having the advantages of high strength and high corrosion resistance of the amorphous alloy itself. The influence of alloying elements and interstitial elements on the organization and properties of the alloy is analyzed as follows:

[0017] There is at least one group of atomic pairs with positive mixing enthalpy (or mixing enthalpy is 0) between Ti, Nb or Hf elements and Zr or Cu elements respectively, which makes the addition of Ti, Nb or Hf elements beneficial to the preferential precipitation of body-centered cubic solid solution β-Zr phase in the alloy melt. However, if their addition amount is too high, it will affect the formation of amorphous matrix, so their addition amount is controlled between 0.5 and 4.5 at.%.

[0018] The main role of O, C or B elements in the alloy is to support the Snoek relaxation mechanism. They are dissolved in the atomic gaps of the body-centered cubic second phase and the amorphous matrix components, and will undergo reciprocating motion under stress induction, making the amorphous-based composite material exhibit high damping performance. However, excessive addition will lead to a sharp decrease in the amorphous forming ability of the alloy matrix, so their content is controlled in the range of 0.1 to 0.5 at.%.

[0019] The advantages and beneficial effects of the present invention are:

[0020] (1) Due to the effect of the Snoek relaxation mechanism induced by the coupling between the body-centered cubic structure second phase and the amorphous matrix, the amorphous-based composite material maintains its own performance advantages while having high damping performance, thereby expanding the application field and scope of amorphous materials.

[0021] (2) Since the material is an amorphous matrix containing solid solution tough phase particles with a body-centered cubic structure, the material has better room temperature plastic deformation ability and fracture strength.

[0022] (3) Since the Snoek relaxation peak temperature in the material is lower than the glass transition temperature of the amorphous matrix, the material is used at the optimal damping temperature. The alloy has excellent organizational stability and is not prone to glass transition or crystallization instability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is the X-ray diffraction spectrum (a) of the alloy material of Example 1 and the backscattered electron image (b) of its structure.

[0024] Figure 2 It is the DSC curve of the alloy material of Example 1.

[0025] Figure 3 It is the internal friction-temperature spectrum of the alloy material of Example 1. DETAILED DESCRIPTION

[0026] The preparation process and implementation effects of the material of the present invention are further described below in conjunction with 6 specific embodiments.

[0027] Example 1 (Zr 63 Nb 0.5 Al9Cu 23 Fe 4.5 ) 99.5 O 0.5

[0028] Commercial Zr, Nb, Fe, Al, Cu and ZrO2 were used as raw materials to prepare the atomic percentage composition (Zr 63 Nb 0.5 Al9Cu 23 Fe 4.5 ) 99.5 O 0.5 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting; the arc melting working current was 260 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 63 Nb 0.5 Al9Cu23 Fe 4.5 ) 99.5 O 0.5 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.2%.

[0029] Step 2: Suction casting of alloy sheet

[0030] Zr 63 Nb 0.5 Al9Cu 23 Fe 4.5 ) 99.5 O 0.5 The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 5Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 360A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0031] The X-ray diffraction test results of the alloy material are as follows Figure 1 As shown in a, the sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image is as follows Figure 1 As shown in (b), it can be observed that the amorphous matrix is ​​distributed with irregularly shaped second phases. Thermal analysis shows that its glass transition temperature is 385°C ( Figure 2 );like Figure 3 The internal friction peak Q is measured by the sub-resonance method. -1 0.015 (0.1Hz)

[0032] Example 2 (Zr 60.5 Nb3Al9Cu 23 Fe 4.5 ) 99.7 O 0.3

[0033] Commercial Zr, Nb, Fe, Al, Cu and ZrO2 were used as raw materials to prepare the atomic percentage composition (Zr 60.5 Nb3Al9Cu 23 Fe 4.5 ) 99.7 O 0.3 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting; the arc melting working current was 260 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 60.5 Nb3Al9Cu 23 Fe 4.5 ) 99.7 O 0.3Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.4%.

[0034] Step 2: Suction casting of alloy sheet

[0035] Zr 60.5 Nb3Al9Cu 23 Fe 4.5 ) 99.7 O 0.3 The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 5Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 360A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0036] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image can be observed to have an irregularly shaped second phase distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 390°C; the sub-resonance method measures its internal friction peak Q -1 0.012 (0.1Hz)

[0037] Example 3 (Zr 59 Nb 4.5 Al9Cu 23 Fe 4.5 ) 99.9 O 0.1

[0038] Commercial Zr, Nb, Fe, Al, Cu and ZrO2 were used as raw materials to prepare the atomic percentage composition (Zr 59 Nb 4.5 Al9Cu 23 Fe 4.5 ) 99.9 O 0.1 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.01-0.10 MPa industrial pure argon gas for melting; the arc melting working current was 290 A, and the melting was repeated 4 times to obtain a uniform composition (Zr 59 Nb 4.5 Al9Cu 23 Fe 4.5 ) 99.9 O 0.1 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.3%.

[0039] Step 2: Suction casting of alloy sheet

[0040] Zr 59 Nb4.5 Al9Cu 23 Fe 4.5 ) 99.9 O 0.1 The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 7Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 380A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0041] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image shows that an irregularly shaped second phase is distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 405°C. The sub-resonance method measures its internal friction peak Q -1 0.011 (0.1Hz)

[0042] Example 3 (Zr 63 Hf 0.5 Al9Cu 23 Fe 4.5 ) 99.9 C 0.1

[0043] Commercial Zr, Hf, Fe, Al, Cu and C are used as raw materials to prepare the atomic percentage composition (Zr 63 Hf 0.5 Al9Cu 23 Fe 4.5 ) 99.9 C 0.1 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting. The arc melting current was 290 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 63 Hf 0.5 Al9Cu 23 Fe 4.5 ) 99.9 C 0.1 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.3%.

[0044] Step 2: Suction casting of alloy sheet

[0045] Zr 63 Hf 0.5 Al9Cu 23 Fe 4.5 ) 99.9 C 0.1The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 7Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 380A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0046] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with β-Zr phase and amorphous matrix. Its backscattered electron image shows that an irregularly shaped second phase is distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 386°C. The sub-resonance method measures its internal friction peak Q -1 0.012 (0.1Hz)

[0047] Example 4 (Zr 59 Hf 4.5 Al9Cu 23 Fe 4.5 ) 99.5 C 0.5

[0048] Commercial Zr, Hf, Fe, Al, Cu and C are used as raw materials to prepare the atomic percentage composition (Zr 59 Hf 4.5 Al9Cu 23 Fe 4.5 ) 99.5 C 0.5 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting. The arc melting current was 290 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 59 Hf 4.5 Al9Cu 23 Fe 4.5 ) 99.5 C 0.5 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.3%.

[0049] Step 2: Suction casting of alloy sheet

[0050] Zr 59 Hf 4.5 Al9Cu 23 Fe 4.5 ) 99.5 C 0.5The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 7Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 380A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0051] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image shows that an irregularly shaped second phase is distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 388°C. The sub-resonance method measures its internal friction peak Q -1 0.014 (0.1Hz)

[0052] Example 5 (Zr 63 Ti 0.5 Al9Cu 23 Fe 4.5 ) 99.9 B 0.1

[0053] Commercial Zr, Ti, Fe, Al, Cu and B are used as raw materials to prepare the atomic percentage composition (Zr 63 Ti 0.5 Al9Cu 23 Fe 4.5 ) 99.9 B 0.1 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting. The arc melting current was 290 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 63 Ti 0.5 Al9Cu 23 Fe 4.5 ) 99.9 B 0.1 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.3%.

[0054] Step 2: Suction casting of alloy sheet

[0055] Zr 63 Ti 0.5 Al9Cu 23 Fe 4.5 ) 99.9 B 0.1The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 6Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 380A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0056] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image shows that an irregularly shaped second phase is distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 390°C. The sub-resonance method measures its internal friction peak Q -1 0.011 (0.1Hz)

[0057] Example 6 (Zr 59 Ti 4.5 Al9Cu 23 Fe 4.5 ) 99.5 B 0.5

[0058] Commercial Zr, Ti, Fe, Al, Cu and B are used as raw materials to prepare the atomic percentage composition (Zr 59 Ti 4.5 Al9Cu 23 Fe 4.5 ) 99.5 B 0.5 The target alloy was prepared by placing the weighed raw materials in a water-cooled copper crucible of an arc melting furnace, and then evacuating to 6 Pa and filling with 0.05 MPa industrial pure argon for melting. The arc melting current was 290 A, and the melting was repeated 4 times to obtain a uniform composition of (Zr 59 Ti 4.5 Al9Cu 23 Fe 4.5 ) 99.5 B 0.5 Alloy ingot. The mass loss rate of alloy ingot before and after smelting is 0.3%.

[0059] Step 2: Suction casting of alloy sheet

[0060] Zr 59 Ti 4.5 Al9Cu 23 Fe 4.5 ) 99.5 B 0.5The alloy ingot was placed in a water-cooled copper crucible for negative pressure suction casting, evacuated to 6Pa, and filled with 0.05MPa of industrial pure argon as a protective gas. Arc melting and copper mold suction casting technology were used. Under an arc working current of 380A, the target alloy ingot was melted and then sucked into the water-cooled copper mold chamber. The mold was cooled to room temperature and taken out to obtain a plate-like sample.

[0061] The X-ray diffraction test results of the alloy material show that the plate-like sample is an amorphous composite material with a β-Zr phase and an amorphous matrix. Its backscattered electron image shows that an irregularly shaped second phase is distributed on the amorphous matrix. Thermal analysis shows that its glass transition temperature is 389°C. The sub-resonance method measures its internal friction peak Q -1 0.015 (0.1Hz)

[0062] The above-described embodiments merely express the implementation methods of the present invention, but they cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A high damping zirconium-based amorphous composite material, characterized in that: The high damping zirconium-based amorphous composite material is a Snoek-type high damping zirconium-based amorphous composite material containing a body-centered cubic structure second phase; The constituent elements include Zr, M, Fe, Al, Cu, and X.

2. The high damping zirconium-based amorphous composite material according to claim 1, characterized in that: The atomic percentage composition formula of the high damping zirconium-based amorphous composite material is: 63.5-a M a Al9Cu 23 Fe 4.5 ) 100-b X b , M=Nb, Ti or Hf, X=O, C or B, where 0.5≤a≤4.5, 0.1≤b≤0.

5.

3. A high damping zirconium-based amorphous composite material according to claim 1 or 2, characterized in that: The damping performance Q of the high damping amorphous composite material is -1 The value is 0.011~0.

015.

4. A method for preparing the high damping zirconium-based amorphous composite material according to claim 1, 2 or 3, characterized in that: The preparation method uses commercial industrial pure Zr, M, Fe, Al, Cu, and N as raw materials, wherein M is Nb, Ti, or Hf, and N is C, B, or ZrO2, and the atomic percentage composition is (Zr 63.5-a M a Al9Cu 23 Fe 4.5 ) 100-b X b The target alloy is then melted into alloy ingots using vacuum arc melting technology, and finally the required alloy material plates are obtained through copper mold casting technology.

5. The method for preparing a high damping zirconium-based amorphous composite material according to claim 4, characterized in that: The following steps are involved: Step 1: Melting of alloy ingots Commercial industrial pure Zr, M, Fe, Al, Cu, N are used as raw materials to prepare the atomic percentage composition (Zr 63.5- a M a Al9Cu 23 Fe 4.5 ) 100-b X b The target alloy is placed in an arc melting furnace, and after vacuuming, industrial pure argon is filled in for melting. The working current of the arc melting is 260-290A, and the melting is repeated for many times to obtain a target alloy ingot with uniform composition; Step 2: Suction casting of alloy sheet The target alloy ingot obtained in step 1 is placed in a water-cooled copper crucible for negative pressure suction casting. After evacuation, industrial pure argon is filled as a protective gas. Arc melting and copper mold suction casting technology are used. Under an arc working current of 360-380A, the target alloy ingot is melted and then sucked into the water-cooled copper mold cavity. The mold is cooled to room temperature and taken out to obtain a plate-like sample.

6. The method for preparing a high damping zirconium-based amorphous composite material according to claim 5, characterized in that: In the step 1, the mass loss rate of the alloy ingot before and after smelting is controlled within 10 / 1000.

7. The method for preparing a high damping zirconium-based amorphous composite material according to claim 5, characterized in that: In the step 1, the pressure is evacuated to 1-10 Pa, and 0.01-0.10 MPa industrial pure argon is introduced for smelting.

8. The method for preparing a high damping zirconium-based amorphous composite material according to claim 5, characterized in that: In the step 2, the vacuum is evacuated to 1-10 Pa, and 0.01-0.10 MPa of industrial pure argon is filled in as a protective gas.

Citation Information

Patent Citations

  • Amorphous alloys on the base of zr and their use

    CN101010440A

  • Zirconium-based amorphous alloy

    CN102965599A

  • Zr61.5Cu21.5Fe5Al12 bulk amorphous alloy resisting Ar ion and proton irradiation, preparation method and application thereof

    CN103060726A

  • Zr-Al-Cu-Fe-Nb block amorphous alloy and preparation method thereof

    CN103556085A

  • Bulk metallic glass forming alloy

    CN103958709A