Welding wire material for gas protection surfacing of high-hardness and high-crack-resistance Cr5 series tool steel and surfacing method
By optimizing the alloy element composition of the Cr5 series welding wire material, a high hardness and high toughness deposited metal structure is formed, which solves the problem of easy cracking and insufficient wear resistance of the oil drill pipe wear-resistant zone weld, and achieves high hardness and crack resistance. It meets the surfacing requirements of oil drill pipes.
Patent Information
- Application Number
- CN202411082712.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Petroleum drill pipe wear-resistant bands are prone to cracks at the beginning and end of the weld and have insufficient wear resistance, which limits its application.
Using Cr5 series martensitic tool steel welding wire material, by optimizing the composition of carbon, chromium, Nb, W, Mo, V, Ni and other alloying elements, a high hardness and high toughness deposited metal structure is formed to ensure that the martensitic structure accounts for More than 90%, and carbide is added to the welding wire to improve wear resistance.
The slag-free gas shielded surfacing material has achieved high hardness, crack resistance and wear resistance. The on-site drill pipe surface surfacing test results showed that no cracks occurred at the head and tail overlap of the annular weld, meeting practical requirements.
Smart Images

Figure CN118789165A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cladding, and in particular relates to a welding wire material for gas shielded cladding of Cr5 series tool steel with high hardness and high crack resistance, and a cladding method. Background Art
[0002] Composite welding is an important branch in the field of welding. It is a welding method that piles welding materials on tools or machine parts to be welded to repair the wear, cracks and other parts of the welded parts. CO2 gas shielded welding is an early developed arc welding technology. It is widely used due to its low cost, high efficiency and easy operation. However, it also has disadvantages in the welding process, such as large spatter and poor forming, which limits its further promotion and application.
[0003] With the increasing complexity of drilling conditions, deepening of drilling depth and other special drilling requirements, the research and development of wear-resistant belts for oil drill pipes has become an important direction that determines the future development trend of drill pipes. At present, the annular wear-resistant belt of oil drill pipes used for gas-shielded surfacing has low toughness and is prone to cracks at the overlap of the weld head and tail. In addition, defects such as insufficient wear resistance are the main reasons that limit the application of wear-resistant belts for drill pipes. Among the surfacing materials, Cr5 is a tool steel material with high hardness, crack resistance and high toughness, and can be surfacing welded on a variety of weldment substrates. This patent optimizes the alloy components of flux-cored welding wires and optimizes the mineral components to newly develop Cr5 oil drill pipe joint wear-resistant belt surfacing slag-free self-protected flux-cored welding wires, which solves the contradiction between the wear resistance and insufficient toughness of traditional wear-resistant welding wires, and studies the process. Summary of the invention
[0004] In view of the above technical status, the present invention aims to provide a slag-free gas shielded cladding welding wire material, which not only has good process performance, but also has high hardness, high toughness and high wear resistance, which can meet the cladding and repair welding requirements of petroleum wear-resistant belts.
[0005] In order to achieve the above purpose, the present invention adopts Cr5 series martensitic tool steel, and mainly considers the matching of hardness and toughness performance, and designs the main alloy elements as follows:
[0006] (1)C
[0007] The main function of C is to form a large number of fine dispersed carbides with Nb, W, Mo, Ti, V, Cr, etc., which greatly improves the hardness, wear resistance and other properties of the cladding metal. At the same time, controlling the amount of carbon content and alloy content is conducive to the control of the organization and carbide distribution.
[0008] (2)Cr
[0009] High chromium content increases the hardenability, oxidation resistance and corrosion resistance of the deposited metal, and can form chromium carbide solid solution with carbon to strengthen the matrix. However, under the influence of high carbon content, the martensite, ferrite and austenite in the deposited metal structure will undergo qualitative changes in the Cr5 tool steel alloy system as the chromium content changes.
[0010] (3)Nb, W, Mo, V, Ni and other alloys
[0011] Alloys such as niobium, vanadium, molybdenum, tungsten, and nickel have a great influence on the metallographic structure of the high-carbon Cr5 series and are important alloys for balancing the proportion of martensite, austenite, and carbide. The present invention optimizes the content of Nb, W, Mo, V, and Ni so that the organization can form a martensite structure accounting for more than 90% and a part of austenite, which is beneficial to the improvement of the toughness of the surfacing metal. At the same time, fine hard phases represented by NbC exist in the microstructure and are dispersedly distributed, thereby improving the hardness and wear resistance of the wear-resistant belt.
[0012] Through the design of the cladding material of the present invention, the deposited metal structure is martensite (≥90%) and a small amount of austenite and ferrite, and a certain amount of carbides are distributed on the matrix. The hardness of the deposited metal of the cladding material in the welded state is greater than or equal to 58HRc, and can even reach more than 60HRc; the V-notch impact toughness is 24J / cm 2 , so it has excellent crack resistance. The results of the on-site drill pipe surface surfacing test show that no cracks are generated at the head and tail overlaps of the annular weld, and it fully meets the practical requirements after being put into operation.
[0013] That is, the technical solution of the present invention is: a high-hardness and high-crack-resistance Cr5-based martensitic gas-shielded cladding welding wire material, characterized in that, in terms of weight percentage, the deposited metal of the welding wire includes the following components:
[0014] C: 0.36%-0.60%;
[0015] Cr: 5.5%-7.0%;
[0016] Nb: 3.0%-5.0%;
[0017] V: 1.2-3.0%;
[0018] Ni: 0.25%-0.6%;
[0019] Mo: 0.2%-1.0%;
[0020] W: 0.2%-1.0%;
[0021] Mn: 0.2%-1%;
[0022] Si: 0.2%-0.6%;
[0023] The balance is Fe and inevitable impurities.
[0024] Preferably, the carbon in the deposited metal comes from high carbon ferrochrome, silicon carbide and graphite in the welding wire. To ensure the quality of the welding wire, the amount of silicon carbide is controlled below 1% of the total amount of welding wire powder, the content of graphite is controlled below 2% of the total amount of welding wire powder, and the total amount of silicon carbide and graphite cannot exceed 2.5% of the total amount of welding wire powder.
[0025] Preferably, at least part of the C element and the Cr element are added to the welding wire material in the form of high-carbon ferrochrome or low-carbon ferrochrome. Further preferably, the C element is also added to the welding wire material in the form of graphite.
[0026] Preferably, the W element is added to the welding wire material in the form of tungsten powder.
[0027] Preferably, the Mo element is added to the welding wire material in the form of molybdenum powder.
[0028] Preferably, the Ni element is added to the welding wire material in the form of nickel powder.
[0029] Preferably, the V element is added to the welding wire material in the form of ferrovanadium.
[0030] Preferably, the Ti element is added to the welding wire material in the form of ferrotitanium.
[0031] Preferably, the Mn element is added to the welding wire material in the form of manganese powder.
[0032] Preferably, the Nb element is added to the welding wire material in the form of ferroniobium.
[0033] Preferably, the Si element is added to the welding wire material in the form of ferrosilicon.
[0034] As an implementation method, the welding wire material comprises the following components by weight percentage:
[0035] Fluorite: 0.2%-1.5%; zirconium silicon powder: 0.4~1.0%; sodium fluoride: 0.1%-1.4%; potassium titanate: 0.1%-1%; 40 titanium iron: 2.5%-5%; lithium carbonate: 0~0.5%; high carbon ferrochrome 15%-25%; low carbon ferrochrome: 15-25%; ferroniobium: 20-35%; ferrovanadium: 12-22%; nickel powder 1.0%-2.4%; molybdenum powder 0.6%-4%; tungsten powder 0.6%-4%; ferrosilicon: 1%-2%; manganese powder 1%-2.4%; graphite 0.1~2%; silicon carbide: 0.1~1.2%; the balance is iron powder.
[0036] Preferably, the Cr content in the high carbon ferrochrome is 64% or more, and the C content is 8% or more.
[0037] Preferably, the Cr content in the low-carbon ferrochrome is 65% or more, and the C content is 0.035% or less.
[0038] Preferably, the Si content in ferrosilicon is 74% or more.
[0039] Preferably, the Ti content in ferrotitanium is 40% or more.
[0040] Preferably, the V content in the ferrovanadium is 50%-70%.
[0041] Preferably, the Nb content in the ferroniobium is 60%-70%.
[0042] Preferably, the zirconium content in the zirconium silicon powder is 1% or more.
[0043] Preferably, the purity of nickel powder, tungsten powder, molybdenum powder, manganese powder, graphite and silicon carbide is above 99%.
[0044] The diameter of the welding wire is not limited, and is preferably 1.2 mm or 1.6 mm.
[0045] The gas used in the gas protection is not limited and includes carbon dioxide, argon, etc.
[0046] The method for gas shielded cladding using the welding wire of the present invention comprises the following steps:
[0047] (1) preheating the wear-resistant drill pipe; preferably, the preheating temperature is not less than 120° C.;
[0048] (2) gas shielded cladding is performed using the welding wire of the present invention;
[0049] Preferably, the gas flow rate is 20-25 ml / min;
[0050] Preferably, the welding current is 180-380A;
[0051] Preferably, the welding voltage is 32-35V;
[0052] (4) subjecting the welded wear-resistant belt to a slow cooling treatment, or a slow cooling and tempering heat treatment;
[0053] Preferably, the slow cooling rate is 55°C / h-75°C / h;
[0054] Preferably, the mixture is slowly cooled to 40°C-60°C and then put into the furnace for tempering heat treatment;
[0055] As a preference, tempering treatment can be selected: the tempering temperature is 530℃-560℃, the constant temperature time is not less than 4h; in the range of room temperature to 100℃, the heating rate is not higher than 40℃ / h; after exceeding 100℃, the heating rate is not higher than 50℃ / h, and the heating is uniform.
[0056] (5) Cool the drill pipe to room temperature after tempering heat treatment.
[0057] Compared with the prior art, the present invention adopts Cr5 series martensitic tool steel as welding wire material for gas shielded cladding; the hardness and carbide are matched by optimizing the carbon content in the welding wire; the wear resistance and toughness are improved by optimizing the alloy content of the welding wire, and the stability of the cladding material is improved; the mineral and compound components are optimized to have good process performance, especially the reduction of spatter and porosity performance; finally, not only good process performance is obtained, but also high hardness, high crack resistance and high resistance to cold and hot fatigue are obtained.
[0058] The hardness of the deposited metal of the cladding material in the welded state is greater than or equal to 58HRc, and can even reach more than 60HRc; the V-notch impact toughness is 24J / cm 2 , so it has excellent crack resistance. The results of the on-site drill pipe surface surfacing test show that there is no crack at the end-to-end overlap of the annular weld, and it fully meets the practical requirements after being put into operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. The features and advantages of the present invention can be more clearly understood by referring to the drawings. The drawings are schematic and should not be understood as limiting the present invention in any way. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0060] Figure 1 This is the metallographic structure diagram of the test plate cover after surfacing treatment with the welding wire material in Example 2. DETAILED DESCRIPTION
[0061] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0062] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0063] Embodiment 1:
[0064] The welding wire composition is: 15 grams of high carbon ferrochrome; 25 grams of low carbon ferrochrome; 20 grams of ferroniobium; 21.2 grams of ferrovanadium; 2 grams of nickel powder; 3.6 grams of molybdenum; 0.8 grams of tungsten powder; 1 gram of manganese powder; 1 gram of 75 ferrosilicon; 1 gram of graphite; 1 gram of silicon carbide; 1.5 grams of fluorite; 0.4 zirconium silicon powder; 0.8 grams of sodium fluoride; 0.2 grams of potassium titanate; 5 grams of ferrotitanium; 0.5 grams of lithium carbonate, with iron as the balance; a total of 100 grams of powder.
[0065] The above welding wire powder is wrapped with a steel strip to make a flux-cored welding wire with a diameter of Φ1.6 mm. The steel strip is ordinary carbon steel strip H08A, with a thickness of 0.4 mm, a width of 14 mm, and a filling rate of 35%.
[0066] Embodiment 2:
[0067] The welding wire composition is: 18 grams of high carbon ferrochrome; 24 grams of low carbon ferrochrome; 26 grams of ferroniobium; 20 grams of ferrovanadium; 2.4 grams of nickel powder; 2.4 grams of molybdenum powder, 1.4 grams of tungsten powder; 1.6 grams of manganese powder; 1.3 grams of 75 ferrosilicon; 2 grams of graphite; 0.1 grams of silicon carbide; 0.8 grams of fluorite; 0.5 zirconium silicon powder; 0.6 grams of sodium fluoride; 0.4 grams of potassium titanate; 4 grams of ferrotitanium; 0.4 grams of lithium carbonate; iron is the balance; a total of 100 grams of powder.
[0068] The above welding wire powder is wrapped with a steel strip to make a flux-cored welding wire with a diameter of Φ1.6 mm. The steel strip is ordinary carbon steel strip H08A, with a thickness of 0.4 mm, a width of 14 mm, and a filling rate of 35%.
[0069] Embodiment 3:
[0070] The welding wire composition is: 20 grams of high carbon ferrochrome; 20 grams of low carbon ferrochrome; 30 grams of ferroniobium; 16 grams of ferrovanadium; 1 gram of nickel powder; 1.2 grams of molybdenum powder, 3.6 grams of tungsten powder; 1.5 grams of manganese powder; 2.8 grams of 75 ferrosilicon; 1.5 grams of graphite; 0.4 grams of silicon carbide; 0.5 grams of fluorite; 0.6 zirconium silicon powder; 1.1 grams of sodium fluoride; 0.6 grams of potassium titanate; 3 grams of ferrotitanium; 0.3 grams of lithium carbonate; iron is the balance; a total of 100 grams of powder.
[0071] The above welding wire powder is wrapped with a steel strip to make a flux-cored welding wire with a diameter of Φ1.6 mm. The steel strip is ordinary carbon steel strip H08A, with a thickness of 0.4 mm, a width of 14 mm, and a filling rate of 35%.
[0072] Embodiment 4:
[0073] The welding wire composition is: 25 grams of high carbon ferrochrome; 8 grams of low carbon ferrochrome; 33.9 grams of ferroniobium; 12 grams of ferrovanadium; 1.2 grams of nickel powder; 0.8 grams of molybdenum powder, 2.3 grams of tungsten powder; 2 grams of manganese powder; 1.9 grams of 75 ferrosilicon; 0.1 grams of graphite; 0.1 grams of silicon carbide; 0.2 grams of fluorite; 0.8 zirconium silicon powder; 0.3 grams of sodium fluoride; 0.8 grams of potassium titanate; 2.6 grams of ferrotitanium; iron is the balance; a total of 100 grams of powder.
[0074] The above welding wire powder is wrapped with a steel strip to make a flux-cored welding wire with a diameter of Φ1.6 mm. The steel strip is ordinary carbon steel strip H08A, with a thickness of 0.4 mm, a width of 14 mm, and a filling rate of 35%.
[0075] The mass percentages of the main alloy components of the deposited metal in the flux-cored welding wires in the above-mentioned Examples 1-4 are shown in Table 1 below.
[0076] Table 1 Mass percentage of main alloy components in the cap cladding material (wt%)
[0077] Example C Cr Nb V Ni Mo W Mn Si Fe 1 0.42 6.5 3 2.65 0.5 0.9 0.2 0.25 0.18 margin 2 0.46 6.8 3.9 2.5 0.6 0.6 0.35 0.38 0.2 margin 3 0.5 6.5 4.5 2 0.25 0.3 0.9 0.375 0.45 margin 4 0.55 5.5 5.1 1.5 0.3 0.2 0.57 0.5 0.38 margin
[0078] The flux-cored welding wire in the above-mentioned embodiment 1-4 was selected to perform gas shielded surfacing welding on a test plate of length×width×height=200mm×400mm×30mm, and the surfacing thickness of one side was 15mm according to the surfacing specimen of YB / T4326-2013. The specific surfacing process is as follows:
[0079] (1) Preheat the sample to 150°C;
[0080] (2) The flux-cored welding wire in Example 1-4 was used for gas shielded cladding, and the cladding parameters were as follows:
[0081] Protective gas: carbon dioxide
[0082] Gas flow rate: 18ml / min
[0083] Welding current I: 290A
[0084] Welding voltage U: 32V;
[0085] (4) The welded sample is slowly cooled at a rate of 60°C / h. After slowly cooling to 60°C, it is put into the furnace for tempering heat treatment at a tempering temperature of 550°C and a constant temperature time of 4.5h.
[0086] (5) After tempering heat treatment, the sample is cooled with the furnace. When the furnace temperature drops to 260℃, it is taken out of the furnace and air-cooled to room temperature.
[0087] The metallographic structure of the sample subjected to the surfacing treatment with the flux-cored wire in Examples 1-4 is martensite (≥90%) and a small amount of austenite and ferrite, with a certain amount of carbides distributed on the matrix. Figure 1 The figure shows the metallographic structure of the test plate cover after surfacing treatment with the welding wire material in Example 2. The deposited metal structure is martensite (≥90%) and a small amount of austenite and ferrite, and a certain amount of carbides are distributed on the matrix.
[0088] According to the specimen and measurement requirements shown in the appendix of YB / T4326-2013, impact specimens were prepared on the cover layer of the test plate and tested. The results are shown in Table 2 below.
[0089] Table 2 Partial mechanical properties of the cap surfacing materials of Examples 1-4 at different temperatures
[0090] state normal temperature normal temperature Mechanical properties Normal temperature impact toughness (AKv) Hardness(HRC) Example 1 27 61.5 Example 2 29 62.9 Example 3 28 59.9 Example 4 26 60.5
[0091] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. High hardness and high crack resistance Cr5 series martensitic tool steel gas shielded cladding welding wire material, characterized in that: The deposited metal of the welding wire includes the following components by weight percentage: C:0.36%-0.60%; Cr:5.5%-7.0%; Nb: 3.0%-5.0%; V:1.2-3.0%; Ni: 0.25%-0.6%; Mo: 0.2%-1.0%; W:0.2%-1.0%; Mn: 0.2%-1%; Si: 0.2%-0.6%.
2. The welding wire material according to claim 1, characterized in that: The carbon in the deposited metal comes from high carbon ferrochrome, silicon carbide and graphite in the welding wire. To ensure the quality of the welding wire, the amount of silicon carbide is controlled below 1% of the total amount of powder in the welding wire, the content of graphite is controlled below 2% of the total amount of welding wire powder, and the total amount of silicon carbide and graphite cannot exceed 2.5% of the total amount of welding wire powder.
3. The welding wire material according to claim 1, characterized in that: The W element is added to the welding wire material using tungsten powder; The Mo element is added to the welding wire material in the form of molybdenum powder; The Ni element is added to the welding wire material in the form of nickel powder; The V element is added to the welding wire material in the form of ferrovanadium; The Mn element is added to the welding wire material in the form of manganese powder; The Nb element is added to the welding wire material in the form of ferroniobium; The Si element is added to the welding wire material in the form of ferrosilicon.
4. The welding wire material according to claim 1, characterized in that: The welding wire material comprises the following components by weight percentage: High carbon ferrochrome 15%-25%; low carbon ferrochrome: 15-25%; ferroniobium: 20-35%; ferrovanadium: 12-22%; nickel powder 1.0%-2.4%; molybdenum powder 0.6%-4%; tungsten powder 0.6%-4%; Ferrosilicon: 1%-2%; manganese powder 1%-2.4%; graphite 0.1-2%; silicon carbide: 0.1-1.2%; fluorite: 0.2%-1.5%; zirconium silicon powder: 0.4-1.0%; sodium fluoride: 0.1%-1.4%; potassium titanate: 0.1%-1%; 40 ferrotitanium: 2.5%-5%; lithium carbonate: 0-0.5%, and the rest is iron.
5. The welding wire material according to claim 4, characterized in that: The Cr content in high carbon ferrochrome is more than 64%, and the C content is more than 8%; The Cr content in low carbon ferrochrome is more than 65% and the C content is less than 0.035%; The Si content in ferrosilicon is more than 74%; The Ti content in ferrotitanium is more than 40%; The V content in ferrovanadium is 50%-70%; The Nb content in ferroniobium is 60%-70%; The purity of nickel powder, tungsten powder, molybdenum powder, manganese powder, graphite and silicon carbide reaches more than 99% respectively.
6. The welding wire material according to claim 1, characterized in that: The diameter of the welding wire material is 1.2 mm or 1.6 mm; The gas in the gas shielding includes one or two of carbon dioxide and argon.
7. The welding wire material according to any one of claims 1 to 6, characterized in that: The hardness of the deposited metal of the welding wire material in the welded state is ≥57HRc or 60HRc.
8. A method for gas shielded cladding using the welding wire material according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Preheat the weldment; (2) using the welding wire material to perform gas shielded cladding; (3) subjecting the welded parts to a slow cooling treatment; (4) Cool the weldment to room temperature.
9. A method for gas shielded cladding using the welding wire material according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) using the welding wire material to perform gas shielded cladding; (2) subjecting the welded parts to slow cooling and tempering heat treatment; (3) Cool the weldment to room temperature.
10. The gas shielded cladding method according to claim 8 or 9, characterized in that: In the step (1), the preheating temperature is not less than 120°C; In the step (2), the gas flow rate is 20-28 ml / min; In the step (2), the welding current is 280-400A; In the step (2), the welding voltage is 32-38V.
Citation Information
Cited By
Surfacing process and device for charging bell
CN120772628A
Impact-wear-resistant flux-cored wire for welding high-manganese steel lining plate and surfacing method
CN121373899A
An impact and wear resistant flux cored wire for welding high manganese steel liner plate and a surfacing method
CN121373899B