A modified polyester film resistant to electrolyte corrosion and its application in composite current collector
By combining PET resin, nanomaterials and functionalizers in the polyester film, a modified polyester film with excellent corrosion resistance is prepared, which solves the problem of insufficient performance of the existing polyester film and achieves higher machinery Mechanical properties and heat-resistant aging properties are suitable for composite fluid-collection applications of lithium-ion batteries.
Patent Information
- Application Number
- CN202411280295.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing polyester films have insufficient corrosion resistance, mechanical and mechanical properties, flame retardant and heat aging resistance in lithium-ion batteries, which limits its service life and improvement of battery performance.
Using PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluoroterephthalene dimethyl alcohol ester, additive, N-(4-cyanine Materials such as base-3-trifluoromethylphenyl)methacrylamide and methylvinylsilicone fluorene are prepared by double-screw extrusion, casting film formation, bidirectional stretching and electron beam radiation. Liquid-corrosive modified polyester film.
It significantly improves the electrolyte corrosion resistance, mechanical and flame retardancy of the modified polyester film, extends the service life, and reduces production costs, making it suitable for continuous large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane materials, and in particular to a modified polyester membrane resistant to electrolyte corrosion and application thereof in a composite current collector. Background Art
[0002] The current collector is one of the indispensable components of lithium-ion batteries. It helps to reduce the internal resistance of lithium-ion batteries and improve the coulombic efficiency, cycle stability and rate performance of the battery. In lithium batteries, the current collector collects and outputs the current generated by the active material and inputs the electrode current to the active material. It can be seen that the performance of the current collector directly affects the cycle life and electrochemical performance of the lithium battery. It is particularly important to develop a current collector with good comprehensive performance and performance stability.
[0003] Composite current collectors are the mainstream products in the current collector market. They are usually prepared by physical vapor deposition by depositing metal materials on the surface of polymer films such as polypropylene, polyethylene and polyester. Compared with traditional current collectors, composite current collectors have the characteristics of low cost, light weight and good internal insulation. These characteristics enable the use of composite current collectors in batteries to reduce the cost of batteries and improve the energy density and safety of batteries. Polymer film is one of the key components of composite current collectors, and the improvement of its comprehensive performance and performance stability is the bottleneck restricting the further development of composite current collectors.
[0004] Compared with other thermoplastics, polyester film (PET film) has the advantages of good light transmittance, excellent mechanical properties, good electrical insulation, weather resistance, weak acid resistance and oil resistance, non-toxicity, good stability against chemicals, easy processing, etc. It is widely used in packaging materials, electrical insulation materials, capacitor films, flexible printed circuit boards, membrane switches and other electronic and mechanical fields, and is one of the preferred materials for composite current collector base films. However, the existing ordinary PET film has insufficient resistance to electrolyte corrosion, poor mechanical properties, flame retardancy and heat aging resistance, and its service life needs to be further extended.
[0005] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN115320206B discloses a composite polyester film and its preparation method and use, including a first polyester layer, a second polyester layer and a third polyester layer, the first polyester layer and the third polyester layer are respectively located on the surface of both sides of the second polyester layer; in terms of mass percentage, the raw materials for preparing the first polyester layer, the second polyester layer and the third polyester layer independently include: 97.0% to 99.9% polyester material and 0.1% to 3.0% additives; the terminal carboxyl content of the polyester material in the first polyester layer and the third polyester layer is 40 to 100 mol / t, and the terminal carboxyl content of the polyester material in the second polyester layer is 5 to 30 mol / t. The composite polyester film constructs a carboxyl-rich polar surface in the first polyester layer and the third polyester layer, thereby effectively improving the adhesion performance of the composite polyester film, and the adhesion performance of the composite polyester film remains basically unchanged after being stored for a period of time. However, its resistance to electrolyte corrosion, mechanical properties, flame retardancy and heat aging resistance all need to be further improved.
[0006] Therefore, the development of a modified polyester film that is resistant to electrolyte corrosion and has excellent mechanical properties, flame retardancy and heat aging resistance, and a long service life meets market demand, has broad market value and application prospects, and is of great significance to promoting the widespread application and further development of polyester films in composite current collectors. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a modified polyester film resistant to electrolyte corrosion, having excellent mechanical properties, flame retardancy and heat aging resistance, and a long service life, and its application in a composite current collector.
[0008] To achieve the above object, the technical solution adopted by the present invention is: a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 3-5 parts of coupling agent, 10-15 parts of nano aluminum phosphate, 5-8 parts of graphene, 15-25 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 4-6 parts of auxiliary agent, 1-3 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, 0.8-1.2 parts of methylvinylsiloxane, and 1-1.5 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0009] Preferably, the PET resin is at least one of China Xiamen Tenglong DSR TL-103 PET resin, Canada AcloCompounders produced PET008L resin, China Hainan Yisheng Petrochemical YS-W01 PET resin.
[0010] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570.
[0011] Preferably, the particle size of the nano aluminum phosphate is 10-80 nm.
[0012] Preferably, there is no special requirement for the source of the graphene. In one embodiment of the present invention, the graphene is prepared according to the method of Example 1 of Chinese invention patent application number 201510061527.X.
[0013] Preferably, the preparation method of the polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst to a high boiling point solvent, stirring at 110-125°C for 1-3 hours to obtain a reaction solution, then adding the reaction solution to a high-pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 135-155°C under normal pressure for 4-6 hours, then reducing the pressure to 10-50 Pa, heating to 255-275°C, stirring and reacting for 12-20 hours while maintaining the temperature and pressure, cooling to room temperature after the reaction is completed, precipitating in water, washing the precipitated polymer with ethanol for 3-6 times, and finally drying in a vacuum dryer at 85-95°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester.
[0014] Preferably, the molar ratio of the pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenediol, catalyst and high boiling point solvent is 1:1:(0.8-1.2):(8-14).
[0015] Preferably, the high boiling point solvent is dimethyl sulfoxide; the catalyst is a mixture of antimony ethylene glycol, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of (1-2):(0.8-1.2):1.
[0016] Preferably, the inert gas is any one of nitrogen, helium, neon and argon.
[0017] Preferably, the auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is (1-3):(2-4).
[0018] Preferably, the antioxidant is at least one of antioxidant 1010 and antioxidant 168; the lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide.
[0019] Another object of the present invention is to provide a method for preparing the modified polyester film resistant to electrolyte corrosion, comprising the following steps:
[0020] Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film;
[0021] Step S2, mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane evenly, adding the mixture into toluene, dispersing the mixture evenly, coating the mixture on the surface of the primary film, irradiating the mixture under an electron beam, drying the mixture at 85-95° C. to a constant weight, washing the mixture with ethanol, and drying the mixture to obtain a modified polyester film resistant to electrolyte corrosion.
[0022] Preferably, the extrusion temperature of the twin-screw extruder in step S1 is 230-260°C.
[0023] Preferably, the stretching temperature of the biaxial stretching in step S1 is 110-120° C., the stretching rate is 120-80 mm / s, the heat setting temperature is 210-230° C., and the stretching ratio is 3:1.
[0024] Preferably, the mass ratio of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide to toluene is 1:(5-8).
[0025] Preferably, the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 10-90 mA, the voltage is 250-550 kV, the radiation dose rate is 6 kGy / h-72 kGy / h, and the absorbed dose is 50 kGy-240 kGy.
[0026] Another object of the present invention is to provide an application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0027] Due to the application of the above technical solution, the present invention has the following beneficial effects:
[0028] (1) The method for preparing the modified polyester film resistant to electrolyte corrosion disclosed in the present invention has simple process, convenient operation and control, no need for special equipment, small capital investment, low energy consumption, high preparation efficiency and yield rate, is suitable for continuous large-scale production, and has high promotion and application value.
[0029] (2) The modified polyester film resistant to electrolyte corrosion disclosed in the present invention comprises the following raw materials in parts by weight: 100 parts of PET resin, 3-5 parts of coupling agent, 10-15 parts of nano aluminum phosphate, 5-8 parts of graphene, 15-25 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 4-6 parts of auxiliary agent, 1-3 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 0.8-1.2 parts of methylvinylsiloxane, and 1-1.5 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane. Through the mutual cooperation between the raw materials, the prepared modified polyester film has excellent resistance to electrolyte corrosion, good mechanical properties, flame retardancy and heat aging resistance, and long service life.
[0030] (3) The modified polyester film resistant to electrolyte corrosion disclosed in the present invention uses PET resin and polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester as a blended substrate, combining the advantages of the two, not only reducing the production cost, but also ensuring excellent electrolyte corrosion resistance, mechanical properties, flame retardancy and heat aging resistance; both belong to the polyester class and have good compatibility, so that the product has good performance stability and long service life. Polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester is prepared by esterification and polycondensation reaction of pyrimidine-4,6-dicarboxylic acid and 2,3,5,6-tetrafluorophenylenedimethanol, and pyrimidine, fluorobenzene and ester structures are introduced into the molecular structure at the same time. These structures further improve the above properties under the multiple effects of electronic effect, steric effect and conjugation effect.
[0031] (4) The modified polyester film resistant to electrolyte corrosion disclosed in the present invention comprises monomers containing unsaturated olefinic bonds, such as N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane, which are grafted by radiation on the surface of the film to form an interpenetrating network structure. At the same time, cyano, fluoromethyl, phenyl, amide, silane and tetraoxaspiroane structures are introduced. Under the multiple effects of electronic effect, steric effect and conjugation effect, these structures make the prepared polyester film have a stronger bonding force with the metal layer, better electrolyte corrosion resistance, flame retardancy and heat aging resistance, and better mechanical properties. DETAILED DESCRIPTION
[0032] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0033] Example 1, a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 3 parts of coupling agent, 10 parts of nano-aluminum phosphate, 5 parts of graphene, 15 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 4 parts of auxiliary agent, 1 part of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 0.8 parts of methylvinylsiloxane, and 1 part of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0034] The PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the coupling agent is silane coupling agent KH550; the particle size of the nano-aluminum phosphate is 10 nm; and the graphene is prepared according to the method of Example 1 of the Chinese invention patent with application number 201510061527.X.
[0035] The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst into a high boiling point solvent, stirring at 110°C for 1 hour to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 135°C under normal pressure for 4 hours, then reducing the pressure to 10 Pa, heating to 255°C, maintaining the temperature and pressure and stirring for 12 hours, and reacting After the reaction is completed, the mixture is cooled to room temperature, precipitated in water, and the precipitated polymer is washed with ethanol for three times, and finally placed in a vacuum dryer and dried at 85°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the molar ratio of pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol, catalyst, and high boiling point solvent is 1:1:0.8:8; the high boiling point solvent is dimethyl sulfoxide; the catalyst is a mixture of ethylene glycol antimony, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of 1:0.8:1; the inert gas is nitrogen. Through GPC testing, the M of the obtained polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester was measured. n =15357 g / mol, M W / M n =1.323; through elemental analysis and calculation, the molar ratio of the structural units introduced by pyrimidine-4,6-dicarboxylic acid and 2,3,5,6-tetrafluorophenylenedimethanol in the polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester is about 1:1, which is the same as the theoretical value.
[0036] The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is 1:2; the antioxidant is antioxidant 1010; and the lubricant is pentaerythritol stearate.
[0037] A method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps:
[0038] Step S1, after PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester and auxiliary agents are uniformly mixed according to weight parts, extruded through a twin-screw extruder, and then cast into a film, and then biaxially stretched and heat-set in sequence to obtain a primary film; the extrusion temperature of the twin-screw extruder is 230° C.; the stretching temperature of the biaxial stretching in step S1 is 110° C., the stretching rate is 120 mm / s, the heat-setting temperature is 210° C., and the stretching ratio is 3:1;
[0039] Step S2, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane are mixed evenly, added into toluene, uniformly dispersed, coated on the surface of the primary film, irradiated under an electron beam, dried at 85° C. to constant weight, washed with ethanol, and dried to obtain a modified polyester film resistant to electrolyte corrosion; the mass ratio of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide to toluene is 1:5; the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 10 mA, the voltage is 250 kV, the radiation dose rate is 6 kGy / h, and the absorbed dose is 50 kGy. Through the weight change before and after the reaction and elemental analysis, it was calculated that the grafting rate of this step was 1.9wt%, grafting rate = (dry weight of modified polyester film resistant to electrolyte corrosion after modification - dry weight of primary film before modification) / dry weight of primary film before modification × 100%); wherein the mass ratio of the structural units introduced by N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane was about 0.98:0.8:0.97;
[0040] An application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0041] Example 2, a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 3.5 parts of coupling agent, 11 parts of nano-aluminum phosphate, 6 parts of graphene, 17 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 4.5 parts of auxiliary agent, 1.5 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 0.9 parts of methylvinylsiloxane, and 1.2 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0042] The PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the coupling agent is silane coupling agent KH560; the particle size of the nano-aluminum phosphate is 30 nm; and the graphene is prepared according to the method of Example 1 of the Chinese invention patent with application number 201510061527.X.
[0043] The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst into a high boiling point solvent, stirring at 115°C for 1.5 hours to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 140°C under normal pressure for 4.5 hours, then reducing the pressure to 20 Pa, heating to 260°C, maintaining the temperature and pressure and stirring for 14 hours, and reacting After completion, the reaction mixture was cooled to room temperature, precipitated in water, and the precipitated polymer was washed with ethanol for 4 times, and finally dried in a vacuum dryer at 87°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the molar ratio of the pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol, catalyst, and high boiling point solvent was 1:1:0.9:10; the high boiling point solvent was dimethyl sulfoxide; the catalyst was a mixture of antimony ethylene glycol, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of 1.2:0.9:1; and the inert gas was helium.
[0044] The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is 1.5:2.5; the antioxidant is antioxidant 168; and the lubricant is ethylene bis stearamide.
[0045] A method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps:
[0046] Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film;
[0047] Step S2, mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane evenly, adding the mixture into toluene, dispersing the mixture evenly, coating the mixture on the surface of the primary film, irradiating the film under an electron beam, drying the film at 87° C. to a constant weight, washing the film with ethanol, and drying the film to obtain a modified polyester film resistant to electrolyte corrosion.
[0048] The extrusion temperature of the twin-screw extruder in step S1 is 240°C; the stretching temperature of the biaxial stretching in step S1 is 113°C, the stretching rate is 110 mm / s, the heat setting temperature is 215°C, and the stretching ratio is 3:1.
[0049] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide and toluene is 1:6; the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 30 mA, the voltage is 350 kV, the radiation dose rate is 20 kGy / h, and the absorbed dose is 100 kGy.
[0050] An application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0051] Example 3, a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 4 parts of coupling agent, 13 parts of nano-aluminum phosphate, 6.5 parts of graphene, 20 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 5 parts of auxiliary agent, 2 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 1 part of methylvinylsilane, and 1.3 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0052] The PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the coupling agent is silane coupling agent KH570; the particle size of the nano-aluminum phosphate is 40nm; and the graphene is prepared according to the method of Example 1 of the Chinese invention patent with application number 201510061527.X.
[0053] The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst into a high boiling point solvent, stirring at 118°C for 2 hours to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 145°C under normal pressure for 5 hours, then reducing the pressure to 30 Pa, heating to 265°C, maintaining the temperature and pressure and stirring for 16 hours, and reacting After completion, the reaction mixture was cooled to room temperature, precipitated in water, and the precipitated polymer was washed with ethanol for 5 times, and finally dried in a vacuum dryer at 90°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the molar ratio of pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol, catalyst, and high boiling point solvent was 1:1:1:11; the high boiling point solvent was dimethyl sulfoxide; the catalyst was a mixture of ethylene glycol antimony, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of 1.5:1:1; and the inert gas was neon.
[0054] The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is 2:3; the antioxidant is antioxidant 1010; and the lubricant is pentaerythritol stearate.
[0055] A method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps:
[0056] Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film;
[0057] Step S2, after evenly mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane, add the mixture into toluene, evenly disperse the mixture, apply the mixture on the surface of the primary film, irradiate the film under an electron beam, dry the film at 90° C. to a constant weight, wash the film with ethanol, and dry the film to obtain a modified polyester film resistant to electrolyte corrosion.
[0058] The extrusion temperature of the twin-screw extruder in step S1 is 245° C.; the stretching temperature of the biaxial stretching in step S1 is 115° C., the stretching rate is 100 mm / s, the heat setting temperature is 220° C., and the stretching ratio is 3:1.
[0059] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide and toluene is 1:6.5; the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 50mA, the voltage is 400kV, the radiation dose rate is 50kGy / h, and the absorbed dose is 130kGy.
[0060] An application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0061] Example 4, a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 4.5 parts of coupling agent, 14 parts of nano-aluminum phosphate, 7.5 parts of graphene, 23 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 5.5 parts of auxiliary agent, 2.5 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 1.1 parts of methylvinylsiloxane, and 1.4 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0062] The PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570 in a mass ratio of 1:2:3; the particle size of the nano aluminum phosphate is 70nm; and the graphene is prepared according to the method of Example 1 of the Chinese invention patent with application number 201510061527.X.
[0063] The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst into a high boiling point solvent, stirring at 123°C for 2.5 hours to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 150°C under normal pressure for 5.5 hours, then reducing the pressure to 40 Pa, heating to 270°C, maintaining the temperature and pressure and stirring for 19 hours, and reacting After completion, the reaction mixture was cooled to room temperature, precipitated in water, and the precipitated polymer was washed with ethanol for 6 times, and finally dried in a vacuum dryer at 93°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the molar ratio of the pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol, catalyst, and high boiling point solvent was 1:1:1.1:13; the high boiling point solvent was dimethyl sulfoxide; the catalyst was a mixture of antimony ethylene glycol, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of 1.8:1.1:1; and the inert gas was argon.
[0064] The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is 2.5:3.5; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 3:5; the lubricant is a mixture of pentaerythritol stearate and ethylene bisstearamide in a mass ratio of 1:3.
[0065] A method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps:
[0066] Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film;
[0067] Step S2, after evenly mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane, add the mixture into toluene, evenly disperse the mixture, apply the mixture on the surface of the primary film, irradiate the film under an electron beam, dry the film at 93° C. to a constant weight, wash the film with ethanol, and dry the film to obtain a modified polyester film resistant to electrolyte corrosion.
[0068] The extrusion temperature of the twin-screw extruder in step S1 is 255° C.; the stretching temperature of the biaxial stretching in step S1 is 118° C., the stretching rate is 90 mm / s, the heat setting temperature is 225° C., and the stretching ratio is 3:1.
[0069] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide to toluene is 1:7.5; the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 80 mA, the voltage is 530 kV, the radiation dose rate is 68 kGy / h, and the absorbed dose is 230 kGy.
[0070] An application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0071] Example 5, a modified polyester film resistant to electrolyte corrosion, comprising the following raw materials in parts by weight: 100 parts of PET resin, 5 parts of coupling agent, 15 parts of nano-aluminum phosphate, 8 parts of graphene, 25 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 6 parts of auxiliary agent, 3 parts of N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, 1.2 parts of methylvinylsilane, and 1.5 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0072] The PET resin is Tenglong DSR TL-103 PET resin from Xiamen, China; the coupling agent is silane coupling agent KH550; the particle size of the nano-aluminum phosphate is 80nm; and the graphene is prepared according to the method of Example 1 of the Chinese invention patent with application number 201510061527.X.
[0073] The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylene glycol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylene glycol and a catalyst into a high boiling point solvent, stirring at 125°C for 3 hours to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, replacing the air in the reactor with an inert gas, then stirring and reacting at 155°C under normal pressure for 6 hours, then reducing the pressure to 50 Pa, heating to 275°C, maintaining the temperature and pressure and stirring for 20 hours, and the reaction result is The reaction mixture was cooled to room temperature after being dried, precipitated in water, and the precipitated polymer was washed with ethanol for 6 times, and finally dried in a vacuum dryer at 95°C to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the molar ratio of pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol, catalyst, and high boiling point solvent was 1:1:1.2:14; the high boiling point solvent was dimethyl sulfoxide; the catalyst was a mixture of ethylene glycol antimony, tetrabutyl titanate, and p-toluenesulfonic acid in a mass ratio of 2:1.2:1; and the inert gas was argon.
[0074] The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is 3:4; the antioxidant is antioxidant 1010; and the lubricant is ethylene bis stearamide.
[0075] A method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps:
[0076] Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film;
[0077] Step S2, mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane evenly, adding the mixture into toluene, dispersing the mixture evenly, coating the mixture on the surface of the primary film, irradiating the mixture under an electron beam, drying the mixture at 95° C. to a constant weight, washing the mixture with ethanol, and drying the mixture to obtain a modified polyester film resistant to electrolyte corrosion.
[0078] The extrusion temperature of the twin-screw extruder in step S1 is 260°C; the stretching temperature of the biaxial stretching in step S1 is 120°C, the stretching rate is 80 mm / s, the heat setting temperature is 230°C, and the stretching ratio is 3:1.
[0079] The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide and toluene is 1:8; the radiation is continuous electron beam radiation, and during the radiation process, the beam current is 90mA, the voltage is 550kV, the radiation dose rate is 72kGy / h, and the absorbed dose is 240kGy.
[0080] An application of the modified polyester film resistant to electrolyte corrosion in a composite current collector.
[0081] Comparative Example 1, a modified polyester film resistant to electrolyte corrosion, is basically the same as Example 1, except that PET resin is used instead of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester.
[0082] Comparative Example 2, a modified polyester film resistant to electrolyte corrosion, is basically the same as Example 1, except that methylvinylsilane and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane are not added.
[0083] In order to further illustrate the beneficial technical effects of the modified polyester film resistant to electrolyte corrosion involved in each embodiment of the present invention, the modified polyester film resistant to electrolyte corrosion involved in Examples 1-5 and Comparative Examples 1-2 was subjected to relevant performance tests; the thickness of each test sample was 6 μm; the test method was as follows:
[0084] (1) Tensile properties: Tensile strength test is carried out according to GB / T 13022-1991.
[0085] (2) Resistance to electrolyte corrosion: The modified polyester film resistant to electrolyte corrosion in each example was immersed in an electrolyte whose weight was 40 times that of the modified polyester film for 24 hours; then the modified polyester film was taken out, and the electrolyte on the surface of the film was absorbed with absorbent paper, and the film was dried at 90°C to constant weight. After cooling to room temperature, the tensile strength was measured again, and the retention rate of the tensile strength was used as the measure. The larger the value, the better the resistance to electrolyte corrosion. The electrolyte was a mixture of ethylene carbonate, diethyl carbonate and methyl ethyl carbonate in a mass ratio of 1:2:1.
[0086] (3) Flame retardancy: tested in accordance with UL94 standard.
[0087] (4) Heat aging resistance: Each modified polyester film product resistant to electrolyte corrosion was placed in hot air at 90°C for artificial accelerated aging for 100 hours. After cooling to room temperature, the tensile strength was measured again. The heat aging resistance was measured by the retention rate of tensile strength. The larger the value, the better the heat aging resistance.
[0088] As can be seen from Table 1, the modified polyester films resistant to electrolyte corrosion involved in the embodiments of the present invention have better mechanical properties, flame retardant properties, electrolyte corrosion resistance and heat aging resistance than the comparative products. The combined use of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, methylvinylsilane and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane is beneficial to improving the above properties.
[0089] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A modified polyester film resistant to electrolyte corrosion, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of PET resin, 3-5 parts of coupling agent, 10-15 parts of nano aluminum phosphate, 5-8 parts of graphene, 15-25 parts of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, 4-6 parts of auxiliary agent, 1-3 parts of N-(4-cyano-3-trifluoromethylphenyl) methacrylamide, 0.8-1.2 parts of methylvinylsiloxane, and 1-1.5 parts of 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane; The method for preparing the modified polyester film resistant to electrolyte corrosion comprises the following steps: Step S1, PET resin, coupling agent, nano aluminum phosphate, graphene, polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenediol ester, and additives are mixed uniformly by weight, extruded through a twin-screw extruder, and then cast into a film, followed by biaxial stretching and heat setting to obtain a primary film; Step S2, mixing N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, methylvinylsilane, and 3,9-divinyl-2,4,8,10-tetraoxaspiro[5.5]undecane uniformly, adding the mixture into toluene, dispersing the mixture uniformly, coating the mixture on the surface of the primary film, irradiating the mixture under an electron beam, drying the mixture at 85-95° C. to a constant weight, washing the mixture with ethanol, and drying the mixture to obtain a modified polyester film resistant to electrolyte corrosion; The radiation is continuous electron beam radiation. During the radiation process, the beam current is 10-90 mA, the voltage is 250-550 kV, the radiation dose rate is 6 kGy / h-72 kGy / h, and the absorbed dose is 50 kGy-240 kGy.
2. The modified polyester film resistant to electrolyte corrosion according to claim 1, characterized in that: The PET resin is at least one of China Xiamen Tenglong DSR TL-103 PET resin, Canada Aclo Compounders PET008L resin, China Hainan Yisheng Petrochemical YS-W01 PET resin; the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the particle size of the nano aluminum phosphate is 10-80nm.
3. The modified polyester film resistant to electrolyte corrosion according to claim 1, characterized in that: The preparation method of polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester comprises the following steps: adding pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenedimethanol and a catalyst into a high boiling point solvent, stirring at 110-125° C. for 1-3 hours to obtain a reaction solution, then adding the reaction solution into a high pressure reactor, closing the feed port after the addition is completed, passing an inert gas to replace the air in the reactor, and then heating the reactor at normal pressure. The reaction was stirred at 135-155° C. for 4-6 hours, and then the pressure was reduced to 10-50 Pa, the temperature was raised to 255-275° C., and the reaction was stirred for 12-20 hours while maintaining the temperature and pressure. After the reaction was completed, the polymer was cooled to room temperature and precipitated in water, and the precipitated polymer was washed with ethanol for 3-6 times, and finally placed in a vacuum dryer and dried at 85-95° C. to constant weight to obtain polypyrimidine-4,6-dicarboxylic acid 2,3,5,6-tetrafluorophenylenedimethanol ester; the high boiling point solvent is dimethyl sulfoxide.
4. The modified polyester film resistant to electrolyte corrosion according to claim 3, characterized in that: The molar ratio of the pyrimidine-4,6-dicarboxylic acid, 2,3,5,6-tetrafluorophenylenediol, catalyst and high boiling point solvent is 1:1:(0.8-1.2):(8-14).
5. The modified polyester film resistant to electrolyte corrosion according to claim 3, characterized in that: The catalyst is a mixture of antimony ethylene glycol, tetrabutyl titanate and p-toluenesulfonic acid in a mass ratio of (1-2):(0.8-1.2):1; the inert gas is any one of nitrogen, helium, neon and argon.
6. The modified polyester film resistant to electrolyte corrosion according to claim 1, characterized in that: The auxiliary agent includes an antioxidant and a lubricant; the mass ratio of the antioxidant to the lubricant is (1-3):(2-4); the antioxidant is at least one of antioxidant 1010 and antioxidant 168; the lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide.
7. The modified polyester film resistant to electrolyte corrosion according to claim 1, characterized in that: The extrusion temperature of the twin-screw extruder in step S1 is 230-260°C; the stretching temperature of the biaxial stretching in step S1 is 110-120°C, the stretching rate is 120-80 mm / s, the heat setting temperature is 210-230°C, and the stretching ratio is 3:
1.
8. The modified polyester film resistant to electrolyte corrosion according to claim 1, characterized in that: The mass ratio of the N-(4-cyano-3-trifluoromethylphenyl)methacrylamide to toluene is 1:(5-8).
9. Use of the modified polyester film resistant to electrolyte corrosion according to any one of claims 1 to 8 in a composite current collector.
Citation Information
Patent Citations
Composite polyester film and its preparation method and use
CN115320206B
Method for preparing graphene
CN104591178A
Anti-fog film material and preparation method thereof
CN113698656A
High and low temperature resistant modified PET material and preparation method thereof
CN117165053A
Aluminum-plastic film capable of preventing electrolyte corrosion and preparation method of aluminum-plastic film
CN117429153A
Cited By
Electrolyte-resistant anti-aging composite current collector base film
CN122146001A
Ageing-resistant high-flame-retardant high-adhesive-force base film for composite current collector and preparation method thereof
CN122278158A
Aging-resistant high-flame-retardant high-adhesion base film for composite current collectors and a preparation method thereof
CN122278158B