Method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron low-sulfur silicon-aluminum micropowder

Through the leaching, stirring and washing treatment of spodumene acid clinker, combined with magnetic separation and flotation technology, the problems of low utilization rate of lithium slag and high iron and sulfur content of silicon-aluminum micropowder in the lithium extraction process of spodumene are solved, achieving It achieves efficient preparation of low-iron, low-sulfur silicon-aluminum micropowder and efficient extraction of lithium, improving the economy and environmental protection of the process.

CN118792502APending Publication Date: 2024-10-18TIANQI LITHIUM CORP +2

Patent Information

Application Number
CN202410776125.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing spodumene lithium extraction process, the high-value comprehensive utilization rate of lithium slag is low, the wastewater utilization efficiency is low, and the lithium extraction efficiency is low. Moreover, the prepared silicon-aluminum micropowder has high iron content and high sulfur content, which limits its use. Application scope.

Method used

Using spodumene acid clinker for leaching, stirring and washing, combined with magnetic separation and flotation technology, low-iron, low-sulfur silicon-aluminum micro-powder is obtained through classification and grinding processes, and the acidity is adjusted through neutralizing materials to reduce lithium ions loss and precipitation of iron and aluminum to achieve efficient extraction and resource utilization of lithium.

Benefits of technology

It improves the extraction rate of lithium and the yield and quality of silicon-aluminum powder, reduces the content of iron and sulfur, simplifies the process, reduces costs, and achieves high-value utilization of lithium slag and comprehensive recovery of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792502A_ABST
    Figure CN118792502A_ABST
Patent Text Reader

Abstract

The invention relates to a method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron low-sulfur silicon-aluminum micro powder, and belongs to the technical field of ore lithium extraction. The method for efficiently extracting lithium from the spodumene acid clinker and preparing the low-iron low-sulfur silicon-aluminum micro powder comprises the following steps: a, mixing the spodumene acid clinker with water, leaching to obtain leached slurry, and carrying out solid-liquid separation on the leached slurry to obtain leached residues 1 and filtrate 1; b, mixing the leaching residues 1 with water, stirring and washing to obtain stirring and washing slurry, and performing solid-liquid separation on the stirring and washing slurry to obtain filtrate 2 and stirring and washing residues 1; and c, mixing the stirring and washing slag 1 with water, carrying out ore grinding and grading operation to obtain fine-fraction slurry, and carrying out a separation process to obtain the low-iron low-sulfur silicon-aluminum micro powder. From overall consideration, a small amount of residual soluble lithium salt in the process of preparing the silicon-aluminum micro powder from the lithium slag is fully recycled, and the problem that the sulfur content in a final product possibly exceeds the standard due to the fact that the concentration of lithium salt in circulating water is gradually increased in the production process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder, belonging to the technical field of lithium extraction from ores. Background Art

[0002] There are two main methods for preparing lithium salts in industry: one is to extract lithium from salt lake brine, and the other is to extract lithium from ores. Most salt lake brines have the characteristics of low lithium content and high magnesium-lithium ratio, which makes development difficult and difficult to implement industrially; while lithium extraction from ores has the advantages of small material flow, high production efficiency, low energy consumption, and high lithium recovery rate. Currently, most lithium is extracted from spodumene as raw material.

[0003] There are two main methods for extracting lithium from spodumene: sulfuric acid method and lime method. The lime method has been less used due to its high energy consumption, high production cost, low recovery rate and other disadvantages. The sulfuric acid method is to first roast the spodumene concentrate at high temperature to convert α-spodumene into β-spodumene, and then grind the calcined β-spodumene and mix it with concentrated sulfuric acid for sulfuric acid roasting to obtain spodumene acid clinker, referred to as spodumene acid clinker. After the acid clinker is cooled, it is leached to generate soluble lithium sulfate and insoluble lithium smelting slag. The pH of the leaching solution is adjusted with lime milk / calcium carbonate, etc., and sodium carbonate is added to remove impurities such as calcium, magnesium, iron, and aluminum to obtain a purified solution of lithium sulfate. The purified solution is carbonized to precipitate lithium to obtain lithium carbonate, and the lithium extraction rate can reach 90%. A large amount of insoluble lithium smelting slag is produced during the lithium extraction process using the sulfuric acid method, which is mainly used in low-quality traditional building materials industries such as cement, concrete, and expanded clay. How to comprehensively recycle and utilize lithium smelting slag in a high-value manner and turn waste into treasure has become an urgent issue, thereby providing a new way to alleviate environmental pressure and solve the bottleneck that restricts the development of the new energy industry chain.

[0004] In the prior art, patent CN108273826A discloses a method for recycling lithium slag in a full phase and high value. The patent obtains pyrophyllite raw materials for glass fiber by slurry adjustment, carbonate reaction, and magnetic separation. The method requires crystallization to recover sulfate products, and has the disadvantages of high cost and low alkali conversion efficiency, making it difficult to achieve industrial application. Patent CN108147658A obtains pyrophyllite raw materials for glass fiber by slurry adjustment, physical ore dressing desulfurization, magnetic separation and iron removal. The pyrophyllite for glass fiber produced by this method has the characteristics of high iron and high sulfur, and its application is subject to certain restrictions. Patent CN113976309A discloses a method for comprehensive recovery of lithium, tantalum niobium, silicon aluminum powder, iron concentrate and gypsum from lithium slag. High-purity gypsum concentrate and silicon aluminum powder are obtained by flotation and weak magnetic-strong magnetic separation, and coarse-grained niobium tantalum rich material and coarse-grained iron concentrate are obtained by gravity separation-weak magnetic separation. Patent WO2019 / 141098A1 discloses a method for comprehensive utilization of lithium slag, which firstly makes the sulfate minerals in the lithium slag dispersed and suspended by slurrying and stirring the lithium slag, then desulfurizes it by physical beneficiation, and the obtained desulfurized slurry is subjected to magnetic separation, and finally the magnetic separation slurry obtained by magnetic separation is concentrated, filtered and dried to obtain pyrophyllite raw material for glass fiber. Patent WO2023 / 098500A1 discloses a method for comprehensive recovery of lithium, tantalum niobium, silicon aluminum powder, iron concentrate and gypsum from lithium slag, which obtains coarse-grained tantalum niobium rich material and coarse-grained iron concentrate by re-selecting and weak magnetic separation of lithium slag, and then flotates the re-selection tailings to obtain gypsum and desulfurized slurry, and the desulfurized slurry is then subjected to grinding, weak magnetic separation and strong magnetic separation to obtain silicon aluminum powder products and iron-rich materials, and the iron-rich materials are then subjected to re-selection to obtain tantalum niobium concentrate and high-iron lithium-rich materials. Although lithium slag has been comprehensively utilized in a high-value manner, the silicon aluminum micropowder prepared by the above process has problems such as low yield, complex process, poor separation effect, and poor product quality, which has limited the market application of silicon aluminum micropowder. Secondly, gypsum products have the characteristics of complex process, low purity, and the production of secondary slag, which leads to high production costs and the need to improve economic benefits. In addition, from the patents or papers that have been reported so far, they all focus on the comprehensive resource utilization of lithium slag produced by the existing spodumene lithium extraction process. From a technical perspective, some patents can solve the problem of low sulfur in the preparation of silicon aluminum micropowder from lithium slag (such as: WO2019141098A1, CN108147658A, CN108273826A, CN114226413A, AU2022402780A1, CN113976309A, CN116532235A, CN117065916A), but they cannot solve the problem of high iron content in the preparation of silicon aluminum micropowder, resulting in the use of these technologies to prepare lithium slag into silicon aluminum micropowder. The main reason is due to the defects of the existing spodumene lithium extraction process itself.Patent CN117165787A discloses a method for extracting lithium from spodumene while recovering low-iron and low-sulfur silicon-aluminum powder, high-purity gypsum, tantalum-niobium concentrate and lithium-rich iron material, and can achieve efficient separation of the components. Although it solves the problem of preparing low-iron and low-sulfur silicon-aluminum powder, it does not take the overall situation into consideration, resulting in a waste of a small amount of residual soluble lithium salt in the process of preparing silicon-aluminum powder from lithium slag, and does not solve the problem that the gradual increase in lithium salt concentration in circulating water during the production process may lead to an excessive sulfur content in the final product; at the same time, by adding alkaline substances to the lithium leaching filter residue for slurry adjustment, the processing cost is increased and the raw material consumption is increased, and the purpose of comprehensive resource recovery and utilization of a small amount of soluble lithium salt in the process of preparing silicon-aluminum powder is not achieved.

[0005] In view of this, it is necessary to develop a method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder, so as to solve the problems of low comprehensive utilization rate of waste slag, wastewater utilization, and low lithium extraction efficiency in the existing process of lithium extraction from spodumene concentrate by sulfuric acid method. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a new method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder.

[0007] In order to solve the above technical problems, the method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder of the present invention comprises:

[0008] a. mixing spodumene acid clinker with water and leaching to obtain a leached slurry, wherein the leached slurry is subjected to solid-liquid separation to obtain a leached residue 1 and a filtrate 1;

[0009] b. mixing the leached residue 1 with water and performing a stirring and washing operation to obtain a stirred and washed slurry, and the stirred and washed slurry is subjected to solid-liquid separation to obtain a filtrate 2 and a stirred and washed residue 1;

[0010] c. The stirred and washed slag 1 is mixed with water and subjected to grinding and classification operations to obtain fine-grained slurry, and then subjected to a separation process to obtain low-iron and low-sulfur silicon-aluminum micropowder.

[0011] The method of the present invention has no index requirements for the sulfur, iron and lithium contents of spodumene acid clinker. Under no special conditions, the method can be used to achieve efficient extraction of lithium. At the same time, it is universal and referenceable for the process of extracting lithium from lithium ore using the sulfuric acid method.

[0012] In a specific embodiment, the spodumene acid clinker is an acidified clinker obtained by calcining spodumene concentrate at a high temperature of 1000° C. to 1250° C., cooling and grinding, and acidification and roasting at a temperature of 200 to 300° C.

[0013] In a specific embodiment, the liquid-to-solid ratio of the leaching slurry is 1 to 20:1.

[0014] In a specific implementation manner, the leaching time is 10 to 60 minutes, and the stirring speed of the leaching is 50 to 500 r / min.

[0015] In a specific embodiment, the moisture content of the leached residue 1 is 16-28%.

[0016] In a specific embodiment, the liquid-to-solid ratio of the agitated and washed slurry in step b is 1 to 10:1, preferably the number of agitation and washing is 1 to 4 times, the time for a single agitation and washing is 5 to 120 minutes, and the stirring speed of the agitation and washing is 100 to 1000 r / min; preferably, the filtrate 2 is countercurrently returned to the previous stage agitation and washing operation or directly returned to the leaching operation.

[0017] In a specific embodiment, the water content of the stirred and washed slag 1 in step b is 15-25%.

[0018] In a specific embodiment, the method further includes step b1: washing the stirred and washed slag 1 with water to obtain a washing slurry, obtaining a filtrate 3 and a washing slag 3 after solid-liquid separation of the washing slurry, and then subjecting the washing slag 3 to the grinding and grading operation of step c.

[0019] In a specific embodiment, the mass percentage content of SO3 in the washing residue 3 is lower than 0.60wt%; preferably, the mass percentage content of SO3 in the washing residue 3 is lower than 0.20wt%.

[0020] In a specific embodiment, the liquid-to-solid ratio of the washing slurry in step b1 is 1 to 10:1, preferably the number of washings is 1 to 6 times, the time for a single washing is 5 to 60 minutes, and the stirring speed of the washing is 30 to 500 r / min.

[0021] In a specific embodiment, the filtrate 3 is countercurrently returned to the previous washing operation or directly returned to the stirring washing operation.

[0022] In a specific embodiment, the washing method in step b1 is at least one of ultrasonic washing, pressurized washing, and mechanical stirring washing.

[0023] In a specific embodiment, the water content of the washing residue 3 is 15-24%.

[0024] In a specific embodiment, the grinding and classification operation in step c includes classification and grinding in sequence; preferably, the -325 mesh content in the fine-grained slurry in step c is ≥ 95%; and the slurry concentration of the fine-grained slurry is preferably 20-40%.

[0025] The slurry concentration described in the present invention refers to the percentage of solid mass to the total mass of solid and liquid.

[0026] The grinding and classification operation can be done by grinding first and then classification, or by classification first and then grinding. However, the process of classification first and then grinding reduces the grinding processing volume of lithium slag, reduces the energy consumption of the process, and creates conditions for the subsequent process to produce low-iron and low-sulfur silicon-aluminum micropowder products.

[0027] The -325 mesh refers to particles of 325 mesh or smaller.

[0028] In a specific embodiment, the grinding in step c includes at least one of ball milling, vertical milling and tower milling.

[0029] In a specific embodiment, the concentration of the classified slurry in the grinding and classification operation in step c is 20-60wt%; the slurry concentration of the coarse-grained slurry in the classification operation is 40-70%.

[0030] In a specific embodiment, the classification operation described in step c uses at least one of a hydrocyclone, a hydraulic spiral classifier or a mechanical vibrating screen.

[0031] In a specific embodiment, the separation process includes at least one of magnetic separation and flotation separation.

[0032] In a specific embodiment, the magnetic separation comprises step d. performing weak magnetic separation on the fine-grained slurry to obtain weak magnetic tailings 1 and strong magnetic minerals 1;

[0033] e. The weak magnetic tailings 1 are subjected to strong magnetic separation to obtain strong magnetic tailings 1 and weak magnetic minerals 1;

[0034] f. The strong magnetic tailings 1 are separated into solid and liquid to obtain low-iron and low-sulfur silicon-aluminum powder and filtrate 4; the strong magnetic mineral 1 and the weak magnetic mineral 1 are combined and then separated into solid and liquid to obtain iron-rich material and filtrate 5.

[0035] In a specific embodiment, the slurry concentration of the weak magnetic separation operation in step d is 15-45wt%, and the magnetic field strength is 500-4000Gs; the slurry concentration of the strong magnetic mineral 1 is 1-15wt%, and the slurry concentration of the weak magnetic tailings 1 is 15-40%.

[0036] In a specific embodiment, the slurry concentration of the strong magnetic separation operation in step e is 10-20%, and the magnetic field strength is 0.8-1.6T; the slurry concentration of the strong magnetic tailings 2 is 5-20%, and the slurry concentration of the weak magnetic mineral 2 is 1-10%.

[0037] In a specific embodiment, the moisture content of the low-iron and low-sulfur silicon-aluminum powder in step f is 15-25%, and the moisture content of the iron-rich material is 10-20%.

[0038] In a specific embodiment, the flotation separation method includes mixing the fine-grained slurry with a regulator, a dispersant, and a collector, performing a roughing operation, two scavenging operations, and a fine cleaning operation, and then obtaining low-iron and low-sulfur silicon-aluminum powder and iron-rich material through solid-liquid separation.

[0039] In a specific embodiment, the adjusting agent is at least one of sulfuric acid and sodium hydroxide, and the amount of the adjusting agent is 100-1000 g / t; the dispersing agent is at least one of water glass and sodium hexametaphosphate, and the amount of the dispersing agent is 500-2000 g / t; the collector is at least one of tall oil and sodium petroleum sulfonate, and the amount of the collector is 500-1500 g / t.

[0040] In a specific embodiment, the solid-liquid separation includes: concentration and filtration operations, the concentration equipment is at least one of a high-efficiency concentrator and an inclined plate concentrator, and the filtration equipment is at least one of a plate filter press, a disc filter, a belt filter and a centrifuge.

[0041] In a specific embodiment, the method further includes slurrying the filtrate 1 with a neutralizer to obtain a neutralized slurry, and the neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, and the lithium-rich solution is then subjected to a lithium extraction process to obtain a lithium salt product.

[0042] In the lithium extraction process of step a, the gypsum product obtained by solid-liquid separation after adding a neutralizer to the leachate contains only a small amount of hydroxide colloid. Compared with the gypsum separated from the lithium slag after leaching and neutralization, it is difficult to effectively separate the gypsum completely by the mineral processing method due to the specific porous structure and high adsorption of the lithium slag after leaching and neutralization. The gypsum separated from the solid-liquid after adding a neutralizer to the leachate has the advantages of high purity, good separation effect, simple process flow, etc.

[0043] In a specific embodiment, the neutralizing material is at least one of calcium carbonate, calcium hydroxide and calcium oxide, and the amount of the neutralizing material is preferably 10 to 200 g / L.

[0044] In a specific embodiment, the pH value of the lithium-rich solution is 6-8, and the lithium extraction process is alkalization to remove impurities and carbonization to precipitate lithium.

[0045] In a specific embodiment, the moisture content of the gypsum product is 22-32%.

[0046] In a specific embodiment, the method further comprises returning the filtrate 4 and filtrate 5 to steps c, d, and e for use as water circulation.

[0047] Beneficial effects:

[0048] The present invention takes the overall situation into consideration, fully recovers a small amount of residual soluble lithium salt in the process of preparing silicon aluminum micropowder from lithium slag, solves the problem that the concentration of lithium salt in circulating water gradually increases during the production process, which may lead to excessive sulfur content in the final product; at the same time, no alkaline substances need to be added to the lithium leaching filter residue for slurry adjustment, which is low in cost, and achieves the purpose of comprehensive resource recycling of a small amount of soluble lithium salt in the process of preparing silicon aluminum micropowder. The whole process consumes less raw materials, has a simple process, low cost, and a high lithium leaching rate. At the same time, the silicon aluminum micropowder product obtained has high yield, high quality, and high whiteness.

[0049] Specifically:

[0050] 1. The filter residue obtained by the present invention adopts the "leaching-stirring and washing" or "leaching-stirring and washing-washing process". Compared with the traditional solid-liquid separation after direct leaching and neutralization of acid clinker, the acid concentration in the residue is reduced to weak acidity, the sulfate content in the residue is low, and the lithium ions in the residue are dissolved in the filtrate, which reduces the lithium content in the residue. In the traditional process, calcium oxide, calcium hydroxide or calcium carbonate is added during the leaching and neutralization process, so that the residual acid in the filter residue generates calcium sulfate precipitation, which increases the sulfur content in the filter residue; at the same time, there is a reversible reaction during the leaching and neutralization process. According to the principle of electrolytic electrochemical kinetics, under acidic conditions, the hydrogen ions in the solution replace the lithium ions in the residue. After leaching in the traditional process, due to the continuous decrease in the hydrogen ion concentration and the relative increase in the lithium ion concentration after neutralization, the forward reaction rate is relatively slow, and it is difficult to effectively and efficiently leach lithium, resulting in a low lithium leaching rate and an increase in the lithium content in the residue.

[0051] 2. In the leaching, stirring and washing processes of the present invention, the filtrate adopts a step-by-step countercurrent return process, and the lithium ions in each filtrate can eventually return to the leachate. At the same time, the leachate is strongly acidic, which is beneficial to reduce the reversible reaction of lithium ions, thereby achieving maximum extraction of lithium from spodumene acid clinker and reducing the loss of lithium ions. At the same time, the step-by-step countercurrent return can increase the lithium content in the lithium-rich solution, which is beneficial to the subsequent extraction of lithium salts.

[0052] 3. In the process of the present invention, part of the impurities such as iron and aluminum in the spodumene acid clinker enters the solution, and enters the lithium-rich solution after solid-liquid separation. Under the action of the neutralizer, the acidity of the solution decreases, the pH value increases, and the iron ions and aluminum ions are hydrolyzed to produce hydroxide colloids, which are insoluble in dilute acid. At the same time, the residual acid reacts with the neutralizer to produce calcium sulfate precipitation. After solid-liquid separation, the hydroxide colloid enters the gypsum product along with the calcium sulfate precipitation. This process can effectively avoid the production of hydroxide colloids by iron ions and aluminum ions in the filter residue, which has an adverse effect on the subsequent filter residue to obtain low-iron and low-sulfur silicon-aluminum micropowder products.

[0053] 4. The present invention adopts two sets of water return systems in lithium extraction and preparation of silicon aluminum powder products. In the process of lithium extraction, the water return system can reduce the content of soluble lithium and insoluble lithium oxide in the slag, avoiding the adverse effect of adding alkaline materials on the front-end lithium extraction process in the preparation of silicon aluminum powder products. At the same time, in the front-end leaching-stirring-washing process, a large amount of residual acid enters the solution, and the residual acid content in the filter residue is extremely low. In the back-end filter residue treatment process, there is no need to add alkaline materials for slurry adjustment, and magnetic separation and iron removal are directly performed, which reduces the loss of raw materials and saves processing costs.

[0054] 5. The present invention adopts the process of classification-grinding-magnetic separation, and the iron and sulfur contents in the finally obtained silicon aluminum micropowder are low, wherein the content is less than 0.20% in terms of Fe2O3 and less than 0.20% in terms of SO3. The product has high whiteness, and the obtained silicon aluminum micropowder can be widely used in glass fiber, ceramic fiber, rubber and plastic filler, papermaking and other industries.

[0055] 6. The present invention obtains an iron-rich product while efficiently extracting lithium and preparing a low-iron and low-sulfur silicon-aluminum micropowder product. The iron-rich product is rich in rare metals such as tantalum and niobium. Tantalum-niobium concentrate and beneficiation tailings can be further obtained through a beneficiation method. The tantalum-niobium concentrate can be directly sold as a concentrate product, and the beneficiation tailings can be directly used in the building materials market, realizing a tail-free emission and high-value production process.

[0056] 7. The present invention utilizes spodumene acid clinker to improve lithium recovery efficiency and obtains low-iron and low-sulfur silicon-aluminum micropowder only through a simple mineral processing process, thereby realizing the high-value and resource-based comprehensive utilization of waste slag. The obtained low-iron and low-sulfur silicon-aluminum micropowder product has a high yield, a simple process flow, and a low processing cost, and has great value for industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a process flow chart for extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum powder in Example 1 of the present invention.

[0058] Figure 2 It is a process flow chart of Comparative Examples 1 and 2 of the present invention.

[0059] Figure 3 This is a process flow chart of Comparative Example 3 of the present invention.

[0060] Figure 4 This is a process flow chart of Comparative Example 4 of the present invention.

[0061] Figure 5 Actual pictures of silicon aluminum powder products prepared by the traditional process (A) and the present invention (B). DETAILED DESCRIPTION

[0062] In order to solve the above technical problems, the method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder of the present invention comprises:

[0063] a. mixing spodumene acid clinker with water and leaching to obtain a leached slurry, wherein the leached slurry is subjected to solid-liquid separation to obtain a leached residue 1 and a filtrate 1;

[0064] b. mixing the leached residue 1 with water and performing a stirring and washing operation to obtain a stirred and washed slurry, and the stirred and washed slurry is subjected to solid-liquid separation to obtain a filtrate 2 and a stirred and washed residue 1;

[0065] c. The stirred and washed slag 1 is mixed with water and subjected to grinding and classification operations to obtain fine-grained slurry, and then subjected to a separation process to obtain low-iron and low-sulfur silicon-aluminum micropowder.

[0066] The method of the present invention has no index requirements for the sulfur, iron and lithium contents of spodumene acid clinker. Under no special conditions, the method can be used to achieve efficient extraction of lithium. At the same time, it is universal and referenceable for the process of extracting lithium from lithium ore using the sulfuric acid method.

[0067] In a specific embodiment, the spodumene acid clinker is an acidified clinker obtained by calcining spodumene concentrate at a high temperature of 1000° C. to 1250° C., cooling and grinding, and acidification and roasting at a temperature of 200 to 300° C.

[0068] In a specific embodiment, the liquid-to-solid ratio of the leaching slurry is 1 to 20:1.

[0069] In a specific implementation manner, the leaching time is 10 to 60 minutes, and the stirring speed of the leaching is 50 to 500 r / min.

[0070] In a specific embodiment, the moisture content of the leached residue 1 is 16-28%.

[0071] In a specific embodiment, the liquid-to-solid ratio of the agitated and washed slurry in step b is 1 to 10:1, preferably the number of agitation and washing is 1 to 4 times, the time for a single agitation and washing is 5 to 120 minutes, and the stirring speed of the agitation and washing is 100 to 1000 r / min; preferably, the filtrate 2 is countercurrently returned to the previous stage agitation and washing operation or directly returned to the leaching operation.

[0072] In a specific embodiment, the water content of the stirred and washed slag 1 in step b is 15-25%.

[0073] In a specific embodiment, the method further includes step b1: washing the stirred and washed slag 1 with water to obtain a washing slurry, obtaining a filtrate 3 and a washing slag 3 after solid-liquid separation of the washing slurry, and then subjecting the washing slag 3 to the grinding and grading operation of step c.

[0074] In a specific embodiment, the mass percentage content of SO3 in the washing residue 3 is lower than 0.60wt%; preferably, the mass percentage content of SO3 in the washing residue 3 is lower than 0.20wt%.

[0075] In a specific embodiment, the liquid-to-solid ratio of the washing slurry in step b1 is 1 to 10:1, preferably the number of washings is 1 to 6 times, the time for a single washing is 5 to 60 minutes, and the stirring speed of the washing is 30 to 500 r / min.

[0076] In a specific embodiment, the filtrate 3 is countercurrently returned to the previous washing operation or directly returned to the stirring washing operation.

[0077] In a specific embodiment, the washing method in step b1 is at least one of ultrasonic washing, pressurized washing, and mechanical stirring washing.

[0078] In a specific embodiment, the water content of the washing residue 3 is 15-24%.

[0079] In a specific embodiment, the grinding and classification operation in step c includes classification and grinding in sequence; preferably, the -325 mesh content in the fine-grained slurry in step c is ≥ 95%; and the slurry concentration of the fine-grained slurry is preferably 20-40%.

[0080] The slurry concentration described in the present invention refers to the percentage of solid mass to the total mass of solid and liquid.

[0081] The grinding and classification operation can be done by grinding first and then classification, or by classification first and then grinding. However, the process of classification first and then grinding reduces the grinding processing volume of lithium slag, reduces the energy consumption of the process, and creates conditions for the subsequent process to produce low-iron and low-sulfur silicon-aluminum micropowder products.

[0082] The -325 mesh refers to particles of 325 mesh or smaller.

[0083] In a specific embodiment, the grinding in step c includes at least one of ball milling, vertical milling and tower milling.

[0084] In a specific embodiment, the concentration of the classified slurry in the grinding and classification operation in step c is 20-60wt%; the slurry concentration of the coarse-grained slurry in the classification operation is 40-70%.

[0085] In a specific embodiment, the classification operation described in step c uses at least one of a hydrocyclone, a hydraulic spiral classifier or a mechanical vibrating screen.

[0086] In a specific embodiment, the separation process described in step c includes at least one of magnetic separation and flotation separation.

[0087] In a specific embodiment, the magnetic separation comprises step d. performing weak magnetic separation on the fine-grained slurry to obtain weak magnetic tailings 1 and strong magnetic minerals 1;

[0088] e. The weak magnetic tailings 1 are subjected to strong magnetic separation to obtain strong magnetic tailings 1 and weak magnetic minerals 1;

[0089] f. The strong magnetic tailings 1 are separated into solid and liquid to obtain low-iron and low-sulfur silicon-aluminum powder and filtrate 4; the strong magnetic mineral 1 and the weak magnetic mineral 1 are combined and then separated into solid and liquid to obtain iron-rich material and filtrate 5.

[0090] In a specific embodiment, the slurry concentration of the weak magnetic separation operation in step d is 15-45wt%, and the magnetic field strength is 500-4000Gs; the slurry concentration of the strong magnetic mineral 1 is 1-15wt%, and the slurry concentration of the weak magnetic tailings 1 is 15-40%.

[0091] In a specific embodiment, the slurry concentration of the strong magnetic separation operation in step e is 10-20%, and the magnetic field strength is 0.8-1.6T; the slurry concentration of the strong magnetic tailings 2 is 5-20%, and the slurry concentration of the weak magnetic mineral 2 is 1-10%.

[0092] In a specific embodiment, the moisture content of the low-iron and low-sulfur silicon-aluminum powder in step f is 15-25%, and the moisture content of the iron-rich material is 10-20%.

[0093] In a specific embodiment, the flotation separation method includes mixing the fine-grained slurry with a regulator, a dispersant, and a collector, performing a roughing operation, two scavenging operations, and a fine cleaning operation, and then obtaining low-iron and low-sulfur silicon-aluminum powder and iron-rich material through solid-liquid separation.

[0094] In a specific embodiment, the adjusting agent is at least one of sulfuric acid and sodium hydroxide, and the amount of the adjusting agent is 100-1000 g / t; the dispersing agent is at least one of water glass and sodium hexametaphosphate, and the amount of the dispersing agent is 500-2000 g / t; the collector is at least one of tall oil and sodium petroleum sulfonate, and the amount of the collector is 500-1500 g / t.

[0095] In a specific embodiment, the solid-liquid separation includes: concentration and filtration operations, the concentration equipment is at least one of a high-efficiency concentrator and an inclined plate concentrator, and the filtration equipment is at least one of a plate filter press, a disc filter, a belt filter and a centrifuge.

[0096] In a specific embodiment, the method further includes slurrying the filtrate 1 with a neutralizer to obtain a neutralized slurry, and the neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, and the lithium-rich solution is then subjected to a lithium extraction process to obtain a lithium salt product.

[0097] In the lithium extraction process of step a, the gypsum product obtained by solid-liquid separation after adding a neutralizer to the leachate contains only a small amount of hydroxide colloid. Compared with the gypsum separated from the lithium slag after leaching and neutralization, it is difficult to effectively separate the gypsum completely by the mineral processing method due to the specific porous structure and high adsorption of the lithium slag after leaching and neutralization. The gypsum separated from the solid-liquid after adding a neutralizer to the leachate has the advantages of high purity, good separation effect, simple process flow, etc.

[0098] In a specific embodiment, the neutralizing material is at least one of calcium carbonate, calcium hydroxide and calcium oxide, and the amount of the neutralizing material is preferably 10 to 200 g / L.

[0099] In a specific embodiment, the pH value of the lithium-rich solution is 6-8, and the lithium extraction process is alkalization to remove impurities and carbonization to precipitate lithium.

[0100] In a specific embodiment, the moisture content of the gypsum product is 22-32%.

[0101] In a specific embodiment, the method further comprises returning the filtrate 4 and filtrate 5 to steps c, d, and e for use as water circulation.

[0102] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0103] Example 1

[0104] The spodumene acid clinker used in the embodiments of the present invention and the comparative examples is an acidified clinker obtained by calcining spodumene concentrate at 1000°C to 1250°C, cooling and grinding, and acidification and roasting at 200 to 300°C. The main mineral components are spodumene, albite, potassium feldspar, and quartz, and the main element components are shown in Table 1 below:

[0105] Table 1 Chemical multi-element analysis of spodumene acid clinker

[0106] Components <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[SO3]]> CaO <![CDATA[Fe2O3]]> <![CDATA[Na2O]]> <![CDATA[K2O]]> <![CDATA[Li2O]]> <![CDATA[P2O5]]> MgO <![CDATA[TiO2]]> other Content / wt% 48.58 17.38 14.91 0.35 0.64 0.47 0.46 4.54 0.20 0.11 0.03 12.34

[0107] The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder is described in detail in the process flow. Figure 1 , including the following steps:

[0108] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 22%. The leaching process conditions were as follows: liquid-solid ratio of 2.5:1, leaching time of 30 min, and stirring speed of the leaching tank of 100 r / min.

[0109] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 26%, and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium carbonate, and the amount used is 100 g / L.

[0110] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 18%, and the stirring and washing operation is terminated when the SO3 content in the stirred and washed residue is lower than 0.60%. The stirring and washing process conditions are: stirring and washing liquid-solid ratio of 2.5:1, stirring and washing time of 15 minutes, stirring speed of the stirring and washing tank of 150 r / min, stirring and washing times of 2 times, the filtrate 2 of the second stirring and washing is returned to the first stirring and washing, and the filtrate 2 of the first stirring and washing is returned to the leaching operation of the previous level.

[0111] (4) The washing residue obtained in step (3) is subjected to mechanical stirring washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 20%. When the SO3 content in the washing residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated. The washing operation process conditions are: washing liquid-solid ratio 2.5:1, washing time 5 minutes, washing tank stirring speed 100 r / min, washing times 2 times, the filtrate 3 of the second washing is returned to the first washing, and the filtrate 3 of the first washing is returned to the previous stirring washing operation.

[0112] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 35%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 60%, and the pulp concentration of the fine-grained slurry is 25%; the grinding adopts a ball mill, and the -325 mesh content in the slurry obtained after grinding is 96%; the pulp concentration of the weak magnetic separation is 25%, the magnetic field strength of the weak magnetic field magnetic separator is 2000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 7%, and the pulp concentration of the weak magnetic tailings is 28%; the pulp concentration of the strong magnetic separation is 15%, the magnetic field strength of the strong magnetic field magnetic separator is 1.0T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 3%, and the pulp concentration of the strong magnetic tailings is 14%; the concentration adopts a high-efficiency thickener for concentration, and the solid-liquid separation adopts a plate and frame filter press. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0113] Example 2

[0114] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0115] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 20%. The leaching process conditions were as follows: liquid-solid ratio 3:1, leaching time 30 min, and stirring speed of the leaching tank 100 r / min.

[0116] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 25% and the lithium-rich solution has a pH of 7.5. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium hydroxide, and the amount used is 80 g / L.

[0117] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 20%, and when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 3:1, stirring and washing time of 15 minutes, stirring speed of the stirring and washing tank of 200 r / min, stirring and washing times of 2 times, and filtrate 2 is returned to the stirring and washing or leaching operation of the previous level in turn.

[0118] (4) The stirred and washed residue obtained in step (3) is subjected to ultrasonic washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 21%. When the SO3 content in the washing residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated. The washing operation process conditions are: washing liquid-solid ratio of 3:1, washing time of 5 minutes, washing tank stirring speed of 75 r / min, washing times of 2 times, and the filtrate 3 is returned to the previous washing operation or stirring and washing operation in turn.

[0119] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 30%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 55%, and the pulp concentration of the fine-grained slurry is 20%; the grinding adopts a ball mill, and the -325 mesh content in the slurry obtained after grinding is 97%; the pulp concentration of the weak magnetic separation is 20%, the magnetic field strength of the weak magnetic field magnetic separator is 3000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 8%, and the pulp concentration of the weak magnetic tailings is 23%; the pulp concentration of the strong magnetic separation is 10%, the magnetic field strength of the strong magnetic field magnetic separator is 1.0T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 2%, and the pulp concentration of the strong magnetic tailings is 9%; the concentration adopts a high-efficiency thickener for concentration, and the solid-liquid separation adopts a plate and frame filter press. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 18% and 16%, respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0120] Example 3

[0121] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0122] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leaching residue and filtrate 1. The moisture content of the leaching residue was 18%. The leaching process conditions were: liquid-solid ratio 2:1, leaching time 20 min, and stirring speed of the leaching tank 50 r / min.

[0123] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 28% and the lithium-rich solution has a pH of 7.0. The lithium solution is subjected to alkalization, impurity removal, and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 60 g / L.

[0124] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, wherein the moisture content of the stirred and washed residue is 16%. When the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the previous level of leaching operation. The stirring and washing process conditions are: stirring and washing liquid-solid ratio of 2:1, stirring and washing time of 15 minutes, stirring speed of the stirring and washing tank of 400 r / min, and stirring and washing times of 2 times.

[0125] (4) The stirred and washed residue obtained in step (3) is subjected to pressure washing and solid-liquid separation operations to obtain washed residue and filtrate 3. The water content of the washed residue is 22%. When the SO3 content in the washed residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated, and the filtrate 3 is returned to the washing operation and the previous stirring and washing operation in sequence. The washing operation process conditions are: washing liquid-solid ratio 2:1, washing time 20 min, washing tank stirring speed 100 r / min, and washing times 2 times.

[0126] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 30%, and the classification operation adopts a spiral classifier for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 50%, and the pulp concentration of the fine-grained slurry is 30%; the grinding adopts a vertical mill, and the -325 mesh content in the slurry obtained after grinding is 98%; the pulp concentration of the weak magnetic separation is 30%, the magnetic field strength of the weak magnetic field magnetic separator is 4000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 10%, and the pulp concentration of the weak magnetic tailings is 35%; the pulp concentration of the strong magnetic separation is 20%, the magnetic field strength of the strong magnetic field magnetic separator is 1.6T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 4%, and the pulp concentration of the strong magnetic tailings is 16%; the concentration adopts an inclined plate concentrator for concentration, and a disc filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0127] Example 4

[0128] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0129] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leaching residue and filtrate 1. The moisture content of the leaching residue was 20%. The leaching process conditions were: liquid-solid ratio of 5:1, leaching time of 60 min, and stirring speed of the leaching tank of 300 r / min.

[0130] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 30% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 20 g / L.

[0131] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 18%, when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the stirring and washing operation and the previous level of leaching operation in sequence, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 5:1, stirring and washing time of 5 minutes, stirring speed of the stirring and washing tank of 100 r / min, and stirring and washing times of 1 time.

[0132] (4) The washing residue obtained in step (3) is subjected to mechanical stirring washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 20%. When the SO3 content in the washing residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated, and the filtrate 3 is returned to the washing operation and the previous stirring washing operation in sequence. The washing operation process conditions are: washing liquid-solid ratio of 5:1, washing time 5 min, washing tank stirring speed of 75 r / min, and washing times of 1 time.

[0133] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 30%, and the classification operation adopts a spiral classifier for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 55%, and the pulp concentration of the fine-grained slurry is 20%; the grinding adopts a tower mill, and the -325 mesh content in the slurry obtained after grinding is 95%; the pulp concentration of the weak magnetic separation is 20%, the magnetic field strength of the weak magnetic field magnetic separator is 2000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 10%, and the pulp concentration of the weak magnetic tailings is 23%; the pulp concentration of the strong magnetic separation is 12%, the magnetic field strength of the strong magnetic field magnetic separator is 1.2T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 3%, and the pulp concentration of the strong magnetic tailings is 14%; the concentration adopts an inclined plate concentrator for concentration, and a disc filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 16%, respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0134] Example 5

[0135] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0136] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 21%. The leaching process conditions were as follows: liquid-solid ratio 3:1, leaching time 30 min, and stirring speed of the leaching tank 100 r / min.

[0137] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 26% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 20 g / L.

[0138] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 20%, when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the stirring and washing operation and the previous level of leaching operation in sequence, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 3:1, stirring and washing time of 10 minutes, stirring speed of the stirring and washing tank of 200 r / min, and stirring and washing times of 2 times.

[0139] (4) The stirred washing residue obtained in step (3) is subjected to ultrasonic washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 21%. When the SO3 content in the washing residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated, and the filtrate 3 is returned to the washing operation and the previous stirring washing operation in sequence. The washing operation process conditions are: washing liquid-solid ratio 3:1, washing time 20 min, washing tank stirring speed 150 r / min, and washing times 1 time.

[0140] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 35%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 60%, and the pulp concentration of the fine-grained slurry is 20%; the grinding adopts a tower mill, and the -325 mesh content in the slurry obtained after grinding is 96%; the pulp concentration of the weak magnetic separation is 20%, the magnetic field strength of the weak magnetic field magnetic separator is 3000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 12%, and the pulp concentration of the weak magnetic tailings is 22%; the pulp concentration of the strong magnetic separation is 10%, the magnetic field strength of the strong magnetic field magnetic separator is 1.5T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 1%, and the pulp concentration of the strong magnetic tailings is 12%; the concentration adopts an inclined plate concentrator for concentration, and a disc filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0141] Example 6

[0142] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0143] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 25%. The leaching process conditions were as follows: liquid-solid ratio 4:1, leaching time 40 min, and stirring speed of the leaching tank 250 r / min.

[0144] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 24% and the lithium-rich solution has a pH of 6.5. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 25 g / L.

[0145] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the water content of the stirred and washed residue is 22%, when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the leaching operation of the previous level in sequence, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 4:1, stirring and washing time of 20 minutes, stirring speed of the stirring and washing tank of 200 r / min, and stirring and washing times of 1 time.

[0146] (4) The stirred and washed residue obtained in step (3) is subjected to pressure washing and solid-liquid separation operations to obtain washed residue and filtrate 3. The water content of the washed residue is 22%. When the SO3 content in the washed residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated, and the filtrate 3 is returned to the washing operation and the previous stirring and washing operation in sequence. The washing operation process conditions are: washing liquid-solid ratio 4:1, washing time 10 min, washing tank stirring speed 100 r / min, and washing times 3 times.

[0147] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 25%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 60%, and the pulp concentration of the fine-grained slurry is 25%; the grinding adopts a tower mill, and the -325 mesh content in the slurry obtained after grinding is 98%; the pulp concentration of the weak magnetic separation is 25%, the magnetic field strength of the weak magnetic field magnetic separator is 3000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 10%, and the pulp concentration of the weak magnetic tailings is 26%; the pulp concentration of the strong magnetic separation is 15%, the magnetic field strength of the strong magnetic field magnetic separator is 1.5T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 2%, and the pulp concentration of the strong magnetic tailings is 16%; the concentration adopts an inclined plate concentrator for concentration, and a belt filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 18% and 14%, respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0148] Example 7

[0149] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0150] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 18%. The leaching process conditions were as follows: liquid-solid ratio 2:1, leaching time 60 min, and stirring speed of the leaching tank 300 r / min.

[0151] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 28% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 40 g / L.

[0152] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 18%, when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the stirring and washing operation and the previous level of leaching operation in sequence, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 2:1, stirring and washing time of 30 minutes, stirring speed of the stirring and washing tank of 250 r / min, and stirring and washing times of 2 times.

[0153] (4) The washing residue obtained in step (3) is subjected to ultrasonic washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 18%. When the SO3 content in the washing residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated, and the filtrate 3 is returned to the washing operation and the previous washing operation in sequence. The washing operation process conditions are: washing liquid-solid ratio 2:1, washing time 20 min, washing tank stirring speed 150 r / min, and washing times 3 times.

[0154] (5) The washing residue obtained in step (4) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 25%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 45%, and the pulp concentration of the fine-grained slurry is 20%; the grinding adopts a tower mill, and the -325 mesh content in the slurry obtained after grinding is 98%; the pulp concentration of the weak magnetic separation is 20%, the magnetic field strength of the weak magnetic field magnetic separator is 3000Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 8%, and the pulp concentration of the weak magnetic tailings is 22%; the pulp concentration of the strong magnetic separation is 15%, the magnetic field strength of the strong magnetic field magnetic separator is 1.5T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 2%, and the pulp concentration of the strong magnetic tailings is 16%; the concentration adopts a high-efficiency thickener for concentration, and a centrifuge is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 19% and 15%, respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0155] Example 8

[0156] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0157] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 24%. The leaching process conditions were as follows: liquid-solid ratio 2:1, leaching time 60 min, and stirring speed of the leaching tank 300 r / min.

[0158] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 26% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 40 g / L.

[0159] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, the moisture content of the stirred and washed residue is 22%, when the SO3 content in the stirred and washed residue is lower than 0.60%, the stirring and washing operation is terminated, and the filtrate 2 is returned to the stirring and washing operation and the previous level of leaching operation in sequence, and the stirring and washing process conditions are: stirring and washing liquid-solid ratio of 2:1, stirring and washing time of 30 minutes, stirring speed of the stirring and washing tank of 250 r / min, and stirring and washing times of 2 times.

[0160] (4) The stirred and washed residue obtained in step (3) is subjected to three mechanical stirring washing and solid-liquid separation operations to obtain washing residue and filtrate 3. The water content of the washing residue is 20%. The filtrate 3 is returned to the washing operation and the previous stirring and washing operation in sequence. The three washing process conditions are: washing liquid-solid ratio 2:1, washing time 20 minutes, and washing tank stirring speed of 150r / min.

[0161] (5) The washed residue obtained in step (4) is subjected to pulping, classification, grinding, flotation, concentration, and solid-liquid separation operations. Among them, the pulp concentration of the pulping operation is 28%, the classification operation adopts hydrocyclone for classification, the pulp concentration of the coarse-grained slurry after the classification operation is 50%, and the pulp concentration of the fine-grained slurry is 22%; the grinding adopts tower mill grinding, and the -325 mesh content in the slurry obtained after grinding is 95%; the roughing operation of flotation uses 300g / t of NaOH, 1000g / t of water glass, and 400g / t of tall oil; the scavenging operation I operation of flotation uses 100g / t of adjusting agent, 300g / t of water glass, and 100g / t of tall oil; the scavenging operation II operation of flotation uses 50g / t of adjusting agent, 100g / t of water glass, and 40g / t of tall oil, and the scavenging foam products are returned to the previous level in turn; the water glass dosage of flotation is 400g / t, the selected foam product is iron-rich material, and the selected underflow is returned to the roughing operation. The flotation underflow obtained from the flotation operation is the silicon-aluminum powder, which is concentrated by an inclined plate concentrator, and the solid-liquid separation is carried out by a plate-frame filter press. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The water content of silicon-aluminum powder and iron-rich material is 18% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0162] Example 9

[0163] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0164] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leached residue and filtrate 1. The moisture content of the leached residue was 24%. The leaching process conditions were as follows: liquid-solid ratio 3:1, leaching time 40 min, and stirring speed of the leaching tank 400 r / min.

[0165] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 25% and the lithium-rich solution has a pH of 7.5. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 35 g / L.

[0166] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, wherein the moisture content of the stirred and washed residue is 20%, and the filtrate 2 is returned to the stirring and washing operation and the leaching operation of the previous stage in sequence. When the SO3 content in the stirred and washed residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated. The stirring and washing process conditions are: stirring and washing liquid-solid ratio 4:1, stirring and washing time 20 minutes, stirring speed of the stirring and washing tank 150r / min. The stirring and washing times are 4 times.

[0167] (4) The washing residue obtained in step (3) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 24%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 55%, and the pulp concentration of the fine-grained slurry is 22%; the grinding adopts a ball mill, and the -325 mesh content in the slurry obtained after grinding is 98%; the pulp concentration of the weak magnetic separation is 24%, the magnetic field strength of the weak magnetic field magnetic separator is 1500Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 6%, and the pulp concentration of the weak magnetic tailings is 26%; the pulp concentration of the strong magnetic separation is 18%, the magnetic field strength of the strong magnetic field magnetic separator is 1.2T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 3%, and the pulp concentration of the strong magnetic tailings is 20%; the concentration adopts an inclined plate concentrator for concentration, and a disc filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0168] Example 10

[0169] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0170] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leaching residue and filtrate 1. The moisture content of the leaching residue was 20%. The leaching process conditions were: liquid-solid ratio of 5:1, leaching time of 60 min, and stirring speed of the leaching tank of 300 r / min.

[0171] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 24% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 40 g / L.

[0172] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, wherein the moisture content of the stirred and washed residue is 20%, and the filtrate 2 is returned to the stirring and washing operation and the leaching operation of the previous level in sequence. When the SO3 content in the stirred and washed residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated. The stirring and washing process conditions are: stirring and washing liquid-solid ratio of 5:1, stirring and washing time of 20 minutes, and stirring speed of the stirring and washing tank of 150 r / min. The stirring and washing times are 3 times.

[0173] (4) The washing residue obtained in step (3) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 23%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 45%, and the pulp concentration of the fine-grained slurry is 21%; the grinding adopts a vertical mill, and the -325 mesh content in the slurry obtained after grinding is 96%; the pulp concentration of the weak magnetic separation is 22%, the magnetic field strength of the weak magnetic field magnetic separator is 1800Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 10%, and the pulp concentration of the weak magnetic tailings is 24%; the pulp concentration of the strong magnetic separation is 16%, the magnetic field strength of the strong magnetic field magnetic separator is 1.5T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 2%, and the pulp concentration of the strong magnetic tailings is 18%; the concentration adopts an inclined plate concentrator for concentration, and a belt filter is used for solid-liquid separation. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 21% and 15%, respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0174] Embodiment 11

[0175] A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder comprises the following steps:

[0176] (1) Spodumene acid clinker was leached, and solid-liquid separation was performed to obtain leaching residue and filtrate 1. The moisture content of the leaching residue was 22%. The leaching process conditions were as follows: liquid-solid ratio 4:1, leaching time 40 min, and stirring speed of the leaching tank 250 r / min.

[0177] (2) The filtrate 1 obtained in step (1) is added with a neutralizing material, and the obtained neutralized slurry is subjected to solid-liquid separation to obtain a gypsum product and a lithium-rich solution, wherein the gypsum product has a water content of 24% and the lithium-rich solution has a pH of 7. The lithium-rich solution is subjected to alkalization to remove impurities and carbonization to precipitate lithium to obtain a lithium carbonate product, wherein the neutralizing material is calcium oxide, and the amount used is 50 g / L.

[0178] (3) The leached residue obtained in step (1) is subjected to stirring and washing and solid-liquid separation operations to obtain stirred and washed residue and filtrate 2, wherein the moisture content of the stirred and washed residue is 20%, and the filtrate 2 is returned to the stirring and washing operation and the leaching operation of the previous level in sequence. When the SO3 content in the stirred and washed residue is lower than 0.20%, the washing and solid-liquid separation operations are terminated. The stirring and washing process conditions are: stirring and washing liquid-solid ratio of 6:1, stirring and washing time of 30 minutes, stirring speed of the stirring and washing tank of 120 r / min, and stirring and washing times of 3 times.

[0179] (4) The washing residue obtained in step (3) is subjected to pulping, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and solid-liquid separation. The pulping operation has a pulp concentration of 25%, and the classification operation adopts a hydrocyclone for classification. The pulp concentration of the coarse-grained slurry after the classification operation is 40%, and the pulp concentration of the fine-grained slurry is 20%; the grinding adopts a ball mill, and the -325 mesh content in the slurry obtained after grinding is 98%; the pulp concentration of the weak magnetic separation is 25%, the magnetic field strength of the weak magnetic field magnetic separator is 1500Gs, the pulp concentration of the strong magnetic mineral obtained by the weak magnetic separation is 15%, and the pulp concentration of the weak magnetic tailings is 28%; the pulp concentration of the strong magnetic separation is 15%, the magnetic field strength of the strong magnetic field magnetic separator is 1.3T, the pulp concentration of the weak magnetic mineral obtained by the strong magnetic separation is 4%, and the pulp concentration of the strong magnetic tailings is 16%; the concentration adopts an inclined plate concentrator for concentration, and the solid-liquid separation adopts a plate and frame filter press. Low-iron and low-sulfur silicon-aluminum powder, iron-rich material, filtrate 4 and filtrate 5 are obtained. The moisture contents of the silicon-aluminum powder and the iron-rich material are 20% and 15% respectively. Filtrate 4 and filtrate 5 are returned to the circulating water pool.

[0180] Example 12

[0181] based on Figure 1 , according to the method of Example 1, lithium is extracted and low-iron and sulfur silicon-aluminum powder is prepared, except that during the stirring and washing process, the filtrate is not circulated back to the leaching process and stirring and washing process, and the filtrate after solid-liquid separation in the stirring and washing process is directly treated as wastewater. The washing residue after the stirring and washing process is pulped and then classified, ground, weak magnetic separation, strong magnetic separation, concentrated, and filtered to obtain low-iron and low-sulfur silicon-aluminum powder and iron-rich material.

[0182] Example 13

[0183] based on Figure 1 , according to the method of Example 2, lithium is extracted and low-iron and sulfur silicon-aluminum powder is prepared, except that during the stirring and washing process, the filtrate is not circulated back to the leaching process and stirring and washing process, and the filtrate after solid-liquid separation in the stirring and washing process is directly treated as wastewater. The washing residue after the stirring and washing process is pulped and then classified, ground, weak magnetic separation, strong magnetic separation, concentrated, and filtered to obtain low-iron and low-sulfur silicon-aluminum powder and iron-rich material.

[0184] Comparative Example 1

[0185] based on Figure 2 Lithium is extracted and low-iron and low-sulfur silicon-aluminum powder is prepared according to the method of Example 1. The difference is that after the leaching operation, the leached residue is directly subjected to pulping operation, and after the pulping operation, classification, grinding, weak magnetic separation, strong magnetic separation, concentration and filtration operations are directly carried out to obtain low-iron and low-sulfur silicon-aluminum powder and iron-rich material.

[0186] Comparison column 2

[0187] based on Figure 2 , lithium was extracted and low-iron and low-sulfur silicon-aluminum powder was prepared according to the method of Example 1, except that after the leaching operation, the leached residue was subjected to slurrying / slurry adjustment, and calcium hydroxide was added to adjust the slurry pH to 7.0. After slurry adjustment, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and filtration were performed to obtain low-iron and low-sulfur silicon-aluminum powder and iron-rich material.

[0188] Comparative Example 3

[0189] based on Figure 3 , according to the method of Example 1, lithium is extracted and low-iron and sulfur silicon-aluminum powder is prepared, except that a neutralizer is added to adjust the pH of the leaching slurry to about 7 during the leaching operation, and solid-liquid separation is performed to obtain leaching residue and filtrate 1, filtrate 1 is a lithium-rich solution, and the lithium-rich solution is directly alkalized to remove impurities and carbonized to precipitate lithium to obtain a lithium carbonate product. The leaching residue is stirred, washed, solid-liquid separated, pulped, classified, ground, weak magnetic separation, strong magnetic separation, concentrated, and filtered to obtain low-iron and low-sulfur silicon-aluminum powder and iron-rich material.

[0190] Comparative Example 4

[0191] based on Figure 4 , lithium was extracted and low iron and sulfur silicon aluminum powder was prepared according to the method of Example 1, except that after stirring and washing, calcium hydroxide was added to adjust the slurry pH to 7.0. After slurry adjustment, classification, grinding, weak magnetic separation, strong magnetic separation, concentration, and filtration were performed to obtain low iron and low sulfur silicon aluminum powder and iron-rich material.

[0192] Performance test: Based on the lithium measurement method in GB / T 17413.1-2010 "Chemical analysis method for lithium ore, rubidium ore and cesium ore", the lithium content (in terms of Li2O) in the silicon-aluminum powder and the iron-rich material obtained in Examples 1-13 and Comparative Examples 1-4 was determined;

[0193] Based on GB / T 14506.31-2019 "Chemical analysis methods for silicate rocks Part 31: Determination of 12 components including silicon dioxide by lithium metaborate melt-inductively coupled plasma atomic emission spectrometry", the contents of SiO2, Al2O3, Fe2O3, SO3, CaO, K2O, Na2O, TiO2, Li2O, P2O5 and B2O3 in the silicon aluminum powder in Example 1-13 and Comparative Example 1-4 were determined.

[0194] Based on HJ 816-2016 "Water-soluble cations (Li + 、Na + NH4 + , K + , Ca 2+ Mg 2+ ) Determination of Li in the lithium-rich solution in Examples 1-13 and Comparative Examples 1-4 by ion chromatography+ 、Na + , K + , Ca 2+ and Mg 2+ The content.

[0195] Based on HJ 776-2015 "Determination of 32 elements in water quality - Inductively coupled plasma emission spectrometry", the contents of potassium, sodium, lithium, magnesium, sulfur, silicon, aluminum and calcium in the lithium-rich solutions of Examples 1-13 and Comparative Examples 1-4 were determined.

[0196] The test results of the index content of low iron and low sulfur silicon aluminum powder products in Examples 1-13 and Comparative Examples 1-4 are shown in Table 2. The operating yield of each example = silicon aluminum powder product mass / (silicon aluminum powder product mass+iron-rich material product mass)×100%.

[0197] The test results of the iron-rich material content in Examples 1-13 and Comparative Examples 1-4 are shown in Table 3.

[0198] The test results of gypsum components and contents in Examples 1-13 and Comparative Examples 1-4 are shown in Table 4. The test results of lithium-rich solution indicators in Examples 1-13 and Comparative Examples 1-4 are shown in Table 5.

[0199] Table 2 Test results of index content of low iron and low sulfur silicon aluminum powder products

[0200]

[0201] Table 3 Iron-rich material product index content test results (wt%)

[0202]

[0203]

[0204] Table 4 Gypsum product components and content (wt%)

[0205] Components <![CDATA[SO3]]> CaO <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> <![CDATA[Li2O]]> Example 1 44.67 31.16 0.64 1.98 0.43 0.11 Example 2 44.46 31.01 0.73 2.02 0.47 0.06 Example 3 44.13 30.78 0.71 1.96 0.42 0.08 Example 4 43.92 30.63 0.70 1.97 0.46 0.07 Example 5 44.08 30.74 0.66 2.01 0.44 0.08 Example 6 43.97 30.69 0.68 1.94 0.45 0.09 Example 7 44.15 30.80 0.65 2.02 0.43 0.08 Example 8 44.24 30.84 0.71 2.00 0.47 0.10 Example 9 43.98 30.68 0.69 2.17 0.46 0.08 Example 10 44.12 30.77 0.61 2.03 0.49 0.09 Embodiment 11 44.06 30.63 0.63 2.27 0.47 0.08 Example 12 44.18 30.82 0.69 1.98 0.48 0.09 Example 13 44.22 30.78 0.63 1.94 0.45 0.08 Comparative Example 1 44.09 30.71 0.64 2.08 0.45 0.08 Comparative Example 2 44.11 30.75 0.66 2.12 0.43 0.10 Comparative Example 3 / / / / / / Comparative Example 4 43.96 30.66 0.68 1.97 0.46 0.08

[0206] Table 5 Lithium-rich solution index test results

[0207]

[0208]

[0209] In Examples 1 to 8, parameters such as leaching concentration, stirring times, and washing times are adjusted. In Examples 9 to 11, washing is not performed after stirring and washing. In Examples 12 to 13, the filtrate after stirring and washing and solid-liquid separation in washing is not returned step by step for use. As can be seen from Table 2-5, the sulfur content and iron content in the silicon aluminum micropowder products obtained in Examples 1 to 13 in Table 2 are lower than those in Comparative Examples 1 to 4, indicating that stirring and washing after spodumene acid clinker is leached and lithium extracted can effectively reduce the sulfur content in the silicon aluminum micropowder product. Due to the solid-liquid separation and stirring and washing solid-liquid separation process of leaching, the free iron in the leachate can be reduced to react with the minerals in the filter residue to produce precipitation remaining on the surface of the mineral particles, and the iron content of the silicon aluminum micropowder obtained after weak magnetic separation and strong magnetic separation is low. In Table 3, the content of each element in the lithium-rich iron material obtained by Example 1-13 and Comparative Example 1-4 is not much different, but the sulfur content in Example 1-11 is lower than that in Comparative Example 1-4. After multiple stirring and washing operations, and the filtrate after solid-liquid separation of the stirring and washing operations is returned step by step for use, the sulfur content in the entire product can be reduced.

[0210] In Table 4, there is little difference between the gypsum products obtained from Examples 1-13 and Comparative Examples 1-4, and the purity of the gypsum products is above 94%.

[0211] In Table 5, Li in the lithium-rich solution product of Example 1 + The concentrations are better than those of Comparative Examples 1-4, indicating that multiple stirring and washing and filtrate recycling treatments are beneficial to increasing the content of lithium-rich solution, while reducing lithium loss and improving lithium leaching rate.

[0212] By comparing Example 1 with Comparative Example 1, it can be seen that after the leaching operation, the sulfur content in the slag can be effectively reduced by stirring and washing operations, and finally a low-sulfur silicon-aluminum micropowder product can be obtained.

[0213] By comparing Example 1 and Comparative Example 2, it can be seen that the spodumene acid clinker is directly subjected to solid-liquid separation during leaching, and the obtained leaching residue is directly added with alkaline materials for magnetic separation. Although the iron content in the silicon-aluminum micropowder product can be reduced to 0.27%, the sulfur index is relatively high, and stirring and washing operations can effectively reduce the sulfur content in the filter residue.

[0214] By comparing Example 1 with Comparative Example 3, it can be seen that after adding the neutralizing slurry during the leaching operation and then performing solid-liquid separation, the sulfur content in the filter residue is high after stirring, washing and washing operations, while the filter residue after solid-liquid separation after leaching can achieve good removal of sulfur in the filter residue after stirring, washing and washing operations, indicating that calcium sulfate is formed after adding the neutralizing material, and the solubility of calcium sulfate is low. Only part of the sulfur can be removed by stirring, washing and washing, while adding the neutralizing material to the filtrate after solid-liquid separation can effectively remove the ions (Fe 3+ 、Al 3+ 、SO4 2-It can also prevent the newly generated precipitate or colloid from entering the filter residue and affecting the subsequent desulfurization and iron removal.

[0215] By comparing Example 1 and Comparative Example 4, it can be seen that a low-iron and low-sulfur silicon-aluminum micropowder product can be prepared by adding alkaline materials for slurry adjustment after stirring and washing operations, but the sulfur content in the silicon-aluminum micropowder product obtained in Comparative Example 4 is higher than that in the embodiment, indicating that it is more conducive to obtaining a low-iron and low-sulfur silicon-aluminum micropowder product without slurry adjustment operations, and at the same time it can reduce raw material consumption and save costs.

Claims

1. A method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder, characterized in that: The method comprises: a. mixing spodumene acid clinker with water and leaching to obtain a leached slurry, wherein the leached slurry is subjected to solid-liquid separation to obtain a leached residue 1 and a filtrate 1; b. mixing the leached residue 1 with water and performing a stirring and washing operation to obtain a stirred and washed slurry, and the stirred and washed slurry is subjected to solid-liquid separation to obtain a filtrate 2 and a stirred and washed residue 1; c. The stirred and washed slag 1 is mixed with water and subjected to grinding and classification operations to obtain fine-grained slurry, and then subjected to a separation process to obtain low-iron and low-sulfur silicon-aluminum micropowder.

2. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1, characterized in that: The spodumene acid clinker is an acidified clinker obtained by calcining spodumene concentrate at a high temperature of 1000°C to 1250°C, cooling and grinding, and acidification and roasting at a temperature of 200 to 300°C.

3. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The liquid-to-solid ratio of the leaching slurry is 1 to 20:

1.

4. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The leaching time is 10 to 60 minutes, and the stirring speed of the leaching is 50 to 500 r / min.

5. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The water content of the leached residue 1 is 16-28%.

6. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The liquid-to-solid ratio of the agitated and washed slurry in step b is 1 to 10:1, preferably the agitation and washing is performed 1 to 4 times, the single agitation and washing time is 5 to 120 minutes, and the agitation speed of the agitation and washing is 100 to 1000 r / min; preferably the filtrate 2 is countercurrently returned to the previous agitation and washing operation or directly returned to the leaching operation.

7. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The water content of the stirred and washed slag 1 in step b is 15-25%.

8. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The method further comprises step b1: washing the stirred and washed slag 1 with water to obtain a washing slurry, obtaining a filtrate 3 and a washing slag 3 after solid-liquid separation of the washing slurry, and then subjecting the washing slag 3 to a grinding and classification operation in step c.

9. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 8, characterized in that: The mass percentage content of SO3 in the washing residue 3 is lower than 0.60wt%; preferably, the SO3 content in the washing residue 3 is lower than 0.20wt%.

10. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 8, characterized in that: In step b1, the liquid-to-solid ratio of the washing slurry is 1 to 10:1, preferably the number of washings is 1 to 6 times, the time for a single washing is 5 to 60 minutes, and the stirring speed of the washing is 30 to 500 r / min.

11. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 8, characterized in that: The filtrate 3 is sequentially returned to the previous washing process in countercurrent or directly returned to the stirring washing process.

12. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 8, characterized in that: The washing method in step b1 is at least one of ultrasonic washing, pressurized washing, and mechanical stirring washing.

13. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 8, characterized in that: The water content of the washing residue 3 is 15-24%.

14. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The grinding and classification operation in step c includes classification and grinding in sequence; preferably, the content of -325 mesh in the fine-grained slurry in step c is ≥ 95%; and the slurry concentration of the fine-grained slurry is preferably 20-40%.

15. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The grinding in step c includes at least one of ball milling, vertical milling and tower milling.

16. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The concentration of the classification slurry in the grinding and classification operation in step c is 20-60wt%; the slurry concentration of the coarse-grained slurry in the classification operation is 40-70%.

17. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The classification operation described in step c uses at least one of a hydrocyclone, a hydraulic spiral classifier or a mechanical vibrating screen.

18. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1 or 2, characterized in that: The separation process includes at least one of magnetic separation and flotation separation.

19. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 18, characterized in that: The magnetic separation comprises the step d. subjecting the fine-grained slurry to weak magnetic separation to obtain weak magnetic tailings 1 and strong magnetic minerals 1; e. The weak magnetic tailings 1 are subjected to strong magnetic separation to obtain strong magnetic tailings 1 and weak magnetic minerals 1; f. The strong magnetic tailings 1 are separated into solid and liquid to obtain low-iron and low-sulfur silicon-aluminum powder and filtrate 4; the strong magnetic mineral 1 and the weak magnetic mineral 1 are combined and then separated into solid and liquid to obtain iron-rich material and filtrate 5.

20. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 19, characterized in that: The slurry concentration of the weak magnetic separation operation in step d is 15-45wt%, and the magnetic field strength is 500-4000Gs; the slurry concentration of the strong magnetic mineral 1 is 1-15wt%, and the slurry concentration of the weak magnetic tailings 1 is 15-40%.

21. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 19, characterized in that: The slurry concentration of the strong magnetic separation operation in step e is 10-20%, and the magnetic field strength is 0.8-1.6T; the slurry concentration of the strong magnetic tailings 2 is 5-20%, and the slurry concentration of the weak magnetic mineral 2 is 1-10%.

22. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 19, characterized in that: The moisture content of the low-iron and low-sulfur silicon-aluminum powder in step f is 15-25%, and the moisture content of the iron-rich material is 10-20%.

23. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 18, characterized in that: The flotation separation method comprises mixing fine-grained slurry with a regulator, a dispersant and a collector, performing a roughing operation, two scavenging operations and a fine cleaning operation, and then performing solid-liquid separation to obtain low-iron and low-sulfur silicon-aluminum micropowder and iron-rich material.

24. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 23, characterized in that: The adjusting agent is at least one of sulfuric acid and sodium hydroxide, and the amount of the adjusting agent is 100-1000 g / t; the dispersing agent is at least one of water glass and sodium hexametaphosphate, and the amount of the dispersing agent is 500-2000 g / t; the collecting agent is at least one of tall oil and sodium petroleum sulfonate, and the amount of the collecting agent is 500-1500 g / t.

25. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 19 or 23, characterized in that: The solid-liquid separation includes: concentration and filtration operations, the concentration equipment is at least one of a high-efficiency concentrator and an inclined plate concentrator, and the filtration equipment is at least one of a plate filter press, a disc filter, a belt filter and a centrifuge.

26. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 1, characterized in that: The method also includes slurrying the filtrate 1 with a neutralizer to obtain a neutralized slurry, and obtaining a gypsum product and a lithium-rich solution after solid-liquid separation of the neutralized slurry, and the lithium-rich solution is then subjected to a lithium extraction process to obtain a lithium salt product.

27. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 26, characterized in that: The neutralizing material is at least one of calcium carbonate, calcium hydroxide and calcium oxide, and the amount of the neutralizing material is preferably 10 to 200 g / L.

28. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 26, characterized in that: The pH value of the lithium-rich solution is 6-8, and the lithium extraction process is alkalization to remove impurities and carbonization to precipitate lithium.

29. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 26, characterized in that: The moisture content of the gypsum product is 22-32%.

30. The method for efficiently extracting lithium from spodumene acid clinker and preparing low-iron and low-sulfur silicon-aluminum micropowder according to claim 19, characterized in that: The method further comprises returning the filtrate 4 and filtrate 5 to steps c, d and e for recycling as water.

Citation Information

Patent Citations

  • Method for comprehensively recovering lithium, tantalum-niobium, silicon-aluminum micro-powder, iron ore concentrate and gypsum from lithium slag

    AU2022402780A1

  • High-valued comprehensive utilization method of lithium slag

    CN108147658A

  • Full-phase high-valued recycling method for lithium slag

    CN108273826A

  • Method for comprehensively recovering lithium, tantalum-niobium, silicon-aluminum micro powder, iron ore concentrate and gypsum from lithium slag

    CN113976309A

  • Comprehensive treatment process of lithium slag

    CN114226413A

Cited By

  • Method for synthesizing lithium iron phosphate by spodumene value-added metallurgy

    CN119683591A

  • Method for extracting lithium from spodumene and by-producing low-sulfur lithium smelting slag

    CN119824246A

  • Method for synergistically removing impurities and recycling lithium smelting slag

    CN121669657A