Preparation method and application of denitration-demercuration-cooperated SCR honeycomb catalyst

The honeycomb catalyst prepared by components such as anatase titanium dioxide solves the problem of insufficient oxidation ability of elemental mercury in SCR catalysts in the existing technology, achieves efficient flue gas denitrification and mercury removal effects, and improves the stability of the catalyst properties and compressive strength.

CN118807768AActive Publication Date: 2024-10-22TIANHE BAODING ENVIRONMENTAL ENG +2

Patent Information

Application Number
CN202410791548.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing SCR catalysts have limited ability to oxidize elemental mercury in flue gas, making it difficult to achieve efficient flue gas denitrification and mercury removal, and their SO2/SO3 conversion rate is not high and their stability is poor.

Method used

Using anatase titanium dioxide, pseudo-boehmite, ammonium metavanadate-monoethanolamine aqueous solution, ammonium heptamolybdate, ammonium metatungstate, cerium nitrate, copper nitrate, antimony acetate, glass fiber, lactic acid and polyoxyethylene, etc. component system The prepared honeycomb catalyst is formed through a mixing and extrusion molding process to form a CeO2/CuO/Sb2O3 modified vanadium-titanium-based catalyst structure to improve the activity, mechanical strength and thermal stability of the catalyst.

Benefits of technology

It achieves a removal rate of more than 90% of NOx and Hg0 in flue gas, improves the compressive strength of the catalyst and high-temperature denitration performance, reduces the SO2/SO3 conversion rate, and significantly increases the mercury oxidation rate and the chemically adsorbed oxygen of the catalyst. ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807768A_ABST
    Figure CN118807768A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a denitration-demercuration-cooperated SCR honeycomb catalyst, and relates to the technical field of flue gas denitration. The denitration catalyst is prepared from the following raw material components: anatase type catalytic titanium dioxide, pseudo-boehmite, an ammonium metavanadate-monoethanolamine aqueous solution, ammonium heptamolybdate, ammonium metatungstate, glass fibers, cerous nitrate, copper nitrate, antimony acetate, silica sol, sesbania powder and polyoxyethylene. The prepared denitration and demercuration-cooperated SCR catalyst is large in specific surface area, good in active component dispersity, high in mercury adsorption and oxidation capacity and remarkable in denitration effect, has the good Hg0 oxidation rate and is very suitable for denitration and demercuration emission control of stationary source flue gas of a thermal power plant, a coking plant, a garbage incinerator, a steel sintering machine, a cement kiln and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flue gas denitration, and in particular to a preparation method and application of a denitration and synergistic mercury removal SCR honeycomb catalyst. Background Art

[0002] NOx in the atmosphere mainly comes from the combustion of fossil fuels. The NOx generated by combustion has the characteristics of high emission concentration and concentrated emission locations, so it is difficult to join the nitrogen cycle process, thus causing environmental pollution. At the same time, mercury is also one of the most volatile trace elements in coal, and mercury can seriously endanger life, health and the ecological environment. Therefore, the treatment of nitrogen oxides and mercury pollutants in flue gas is an urgent problem to be solved in the process of sustainable development of industrial production.

[0003] Mercury emissions have attracted widespread attention in recent years due to its volatility, persistence, and bioaccumulation in the environment. Coal-fired power plants are the main anthropogenic source of mercury pollutant emissions. Mercury in coal-fired flue gas exists in the following three forms: elemental mercury (Hg 0 ), calcium mercury oxide (Hg 2+ ) and particle-bound mercury (Hg p ). Among them, Hg 0 It is difficult to be captured by existing pollution control devices (APCD), Hg 2+ and Hg p can be easily removed by wet flue gas desulfurization (WFGD) systems and electrostatic precipitators. 0 Oxidized to Hg 2+ It is of great significance to improve the mercury removal rate.

[0004] Nitrogen oxides (NOx) are an atmospheric pollutant that contributes significantly to acid rain and urban photochemical smog. Selective catalytic reduction (SCR) denitrification systems are widely used by coal-fired power plants around the world to control NOx emissions due to their high efficiency and economic feasibility. Today, the most widely used commercial SCR catalyst is V 2 O 5 / TiO 2 Based catalyst, using tungsten trioxide (WO 3 ) or molybdenum trioxide (MoO 3 ) as a promoter to improve the stability and SO resistance of the catalyst 2 However, the oxidation capacity of existing SCR catalysts for elemental mercury in flue gas is very limited. Therefore, providing an SCR catalyst for denitrification and synergistic demercuration is a technical problem to be solved urgently. Summary of the invention

[0005] The purpose of the present invention is to provide a preparation method and application of a SCR honeycomb catalyst for denitration and synergistic mercury removal, so as to solve the problems existing in the above-mentioned prior art and simultaneously achieve efficient denitration and mercury removal from flue gas.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention is to provide a denitration and mercury removal SCR honeycomb catalyst, comprising the following raw material components in parts by weight:

[0008] 63.5-65 parts of anatase-type catalytic titanium dioxide, 1.0-1.2 parts of pseudo-boehmite, 11-13 parts of ammonium metavanadate-monoethanolamine aqueous solution, 2.0-2.3 parts of ammonium heptamolybdate, 1.3-1.6 parts of ammonium metatungstate, 5-5.5 parts of glass fiber, 1.1-1.5 parts of cerium nitrate, 1.9-2.2 parts of copper nitrate, 1.3-1.6 parts of antimony acetate, 1.5-2.5 parts of silica sol, 0.4-0.8 parts of lactic acid, 0.5-1 parts of sesbania powder and 0.5-1 parts of polyoxyethylene.

[0009] Anatase titanium dioxide mainly contains TiO 2 Composition, specific surface area 100-110m 2 / g, and the particle size distribution D50 ranges from 0.8 to 1.2 μm. It mainly plays the role of catalyst substrate, provides a carrier for the uniform distribution of catalyst active components, and increases N 2 Selective.

[0010] Pseudo-boehmite, mainly composed of Al 2 O 3 ·nH 2 O (n = 0.08-0.62), the main function is to improve the compressive strength of the catalyst.

[0011] The ammonium metavanadate-monoethanolamine aqueous solution is a homogeneous solution obtained by stirring and mixing ammonium metavanadate, monoethanolamine and water at a mass ratio of 1:1:3 at 75°C±5°C; monoethanolamine is a co-solvent for ammonium metavanadate. Ammonium metavanadate is the active component V in the denitration reaction. 2 O 5 The precursor is converted into V after calcination. 2 O 5 , providing active sites for the denitrification reaction.

[0012] The silica sol is 25wt.% of silica sol, and is used together with pseudo-boehmite to improve the mechanical strength of the catalyst.

[0013] Antimony acetate, the main function is to improve the catalyst's resistance to SO 2 performance, reducing SO 2 / SO 3 Conversion rate;

[0014] Cerium nitrate, the main function is to increase the acid content of the catalyst and improve the denitration performance of the catalyst in the high temperature section;

[0015] Copper nitrate, the main function is to improve the oxidation performance of the catalyst and increase the Hg 0 oxidizing capacity.

[0016] The main component of glass fiber is SiO 2 、Al 2 O 3 , CaO, plays a skeleton role in the catalyst and improves the structural strength of the catalyst.

[0017] Lactic acid, adjusts the pH value of the catalyst slurry and mainly improves the plasticity of the material.

[0018] Sesbania powder, with a viscosity range of 850-950mpa.s, is a pore-forming agent that mainly improves the water absorption and water retention of clay and improves the plasticity of clay.

[0019] Polyoxyethylene PEO, with a viscosity range of 250-350mpa.s, plays the role of thickener, flocculant and lubricant to improve the plasticity of mud.

[0020] Ammonium heptamolybdate and ammonium metatungstate are catalyst activity promoters used to improve the catalyst's resistance to sintering, improve the catalyst's thermal stability, and improve the catalyst's resistance to arsenic and alkali metal poisoning.

[0021] As a further preferred embodiment of the present invention, the raw material components of the above-mentioned denitration and synergistic mercury removal SCR honeycomb catalyst also include 3.5-5 parts by mass of ammonia water.

[0022] The second technical solution of the present invention is to provide a method for preparing the above-mentioned denitration and mercury removal SCR honeycomb catalyst, comprising the following steps:

[0023] (1) mixing anatase titanium dioxide, silica sol, pseudo-boehmite and water so that the water content of the system is 38%-39%, and stirring and mixing at 60-80° C. to obtain a mixture A;

[0024] (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to the obtained mixture A, and mixing to obtain a mixture B;

[0025] (3) adjusting the pH value of the mixture B to 8.2-8.5, then adding ammonium heptamolybdate and ammonium metavanadate-monoethanolamine aqueous solution to adjust the water content of the system to 33%-34%, to obtain a mixture C;

[0026] (4) After the mixture C is heated and stirred to adjust the water content of the system to 30-31%, the pH value is adjusted to 7.6-8.0, and glass fiber is added and mixed, and then sesbania powder and polyoxyethylene are added to adjust the water content of the system to 26-29%, and then aged. The aged mud is extruded through a professional extrusion die to extrude the honeycomb catalyst monomer, and then dried and calcined to obtain the denitration and synergistic demercuration SCR honeycomb catalyst.

[0027] The third technical solution of the present invention is to provide another method for preparing a SCR honeycomb catalyst for denitration and synergistic mercury removal, comprising the following steps:

[0028] (1) mixing anatase titanium dioxide, silica sol, pseudo-boehmite and water so that the water content of the system is 38%-39%, and stirring and mixing at 60-80° C. to obtain a mixture A;

[0029] (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to the obtained mixture A, and mixing to obtain a mixture B;

[0030] (3) adding aqueous ammonia to make the pH value of mixture B 8.2-8.5, then adding ammonium heptamolybdate and ammonium metavanadate-monoethanolamine aqueous solution to adjust the water content of the system to 33%-34%, to obtain mixture C;

[0031] (4) The mixture C is heated and stirred, and the water content of the system is adjusted to 30-31%, and then lactic acid is added to adjust the pH value to 7.6-8.0, and then glass fiber is added and mixed, and then sesbania powder and polyoxyethylene are added to adjust the water content of the system to 26-29%, and then aged. The aged mud is extruded through a professional extrusion die to extrude the honeycomb catalyst monomer, and then dried and calcined to obtain the denitration and synergistic demercuration SCR honeycomb catalyst.

[0032] The further preferred preparation process of the present invention is as follows:

[0033] (1) adding anatase titanium dioxide, silica sol, and pseudo-boehmite into a mixer and kneading them uniformly, adding deionized water until the water content is 38%-39%, and mixing and stirring the obtained slurry mixture at 60-80° C. to obtain a mixture A;

[0034] (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to mixture A and mixing them uniformly to obtain mixture B;

[0035] (3) adding ammonia water to the obtained mixture B to adjust the pH value of the reaction system to 8.2-8.5, adding ammonium heptamolybdate and mixing evenly, then adding ammonium metavanadate-monoethanolamine aqueous solution, stirring for 60 minutes, and then heating and dehumidifying until the moisture content of the slurry in the mixer is 33%-34%, thereby obtaining a mixture C;

[0036] (4) The mixture C is heated and stirred, and the water content of the system is adjusted to 30-31%. Lactic acid is added to adjust the pH to 7.6-8.0. Glass fiber is added to the obtained mixture C, and the mud moisture is adjusted to 30-31% after mixing for 40-60 minutes. Then, field sesbania powder and polyoxyethylene are added, and stirring is continued to adjust the moisture content of the mixture to 28%, and the pH value is 7.6-8.0. Then, the mixture is allowed to stand in the mixer for 8-12 hours to obtain aged mud D.

[0037] (5) The aged mud material D is extruded into a strip-shaped mud material through a pre-extruder, and after removing impurities in the mud material, a honeycomb catalyst monomer is extruded through an extrusion die (11-30 holes).

[0038] (6) The extruded honeycomb catalyst monomer is calcined after two-stage drying, the calcination temperature is 500° C., and the calcination time is 35 hours.

[0039] As further preferred embodiment of the present invention, the two-stage drying of the present invention is as follows:

[0040] The primary drying temperature is 30℃-60℃, the humidity is 80-10%, and the drying time is 8 days, which are high humidity and low temperature (humidity 80%-60%, temperature 30℃-40℃), medium humidity and medium temperature (humidity 60%-20%, temperature 40℃-50℃), low humidity and high temperature (humidity 20%-10%, temperature 50℃-60℃); the secondary drying temperature is 60℃ and the time is 24h.

[0041] A fourth technical solution of the present invention is to provide the application of the above-mentioned denitration and synergistic demercuration SCR honeycomb catalyst in flue gas denitration and / or demercuration.

[0042] The content range of the main components in the catalyst of the present invention is as follows: TiO 2 :79-86%;V 2 O 5 :2.2-2.7%;WO 3 :1.4-1.8%;MoO 3 :2.0-2.3%;CeO 2 :0.8-1.2%; CuO:0.7-0.8%; Sb 2 O 3 :0.7-0.9%;SiO 2 :3.7-5.5%;Al 2 O 3 :1.2-1.5%; CaO%: 1.5-2.5%.

[0043] The present invention adopts a mixing extrusion molding process, and prepares a denitrification and mercury removal SCR catalyst through Ce, Cu, and Sb modification and doping, which increases the interaction between the active component and the carrier and increases the chemical adsorption of oxygen O β , forming a catalyst with large specific surface area, good dispersion of active components, and strong mercury adsorption and oxidation ability, which reduces the catalyst's SO 2 The adsorption performance of SCR denitrification and mercury removal overcomes the low oxidation efficiency, poor stability, and SO 2 / SO 3 High conversion rate and other issues.

[0044] The present invention provides a CeO 2 / CuO / Sb 2 O 3 The modified vanadium-titanium honeycomb catalyst structure system introduces an appropriate proportion of SiO 2 and Al 2 O 3 , the mechanical compressive strength of the catalyst is improved (radial compressive strength>0.85MPa, axial compressive strength>3.20MPa). Compared with the traditional vanadium-titanium honeycomb catalyst, the catalyst prepared by the present invention has higher denitration and Hg oxidation performance.

[0045] The denitrification and demercuration principle of the catalyst of the present invention is: the gaseous Hg 0 (Hg g 0 ) first adsorbs on the catalyst surface to form adsorbed Hg 0 (Hg 0 ad ). The redox reaction on the catalyst surface Produce a large amount of chemically adsorbed oxygen and adsorbed Hg 0 It reacts with the abundant chemically adsorbed oxygen on the catalyst surface to generate adsorbed HgO (HgO ad ). The consumed chemically adsorbed oxygen can be recovered through the gaseous O 2 The oxygen vacancies on the catalyst surface are replenished and regenerated, achieving Hg 0 The HgO adsorbed on the catalyst surface will be released into the flue gas after being saturated with adsorption, thus ensuring that the catalyst can oxidize Hg efficiently for a long time. 0 .

[0046] The denitration and mercury removal SCR catalyst prepared by the present invention is suitable for flue gas temperature of 200-380°C, space velocity of 3000 / h-5000 / h, and NOx concentration of 300-650mg / Nm 3 , O 2 The content is 4-16% (volume fraction), SO 2Concentration is 300-500mg / Nm 3 , Hg content is 300-600ng / m 3 When the ammonia-nitrogen molar ratio is 1, a denitrification efficiency of more than 90% can be achieved, and at the same time, the mercury oxidation rate also reaches more than 90%.

[0047] The present invention discloses the following technical effects:

[0048] The denitration and mercury removal SCR catalyst prepared by the present invention has a large specific surface area, good dispersibility of active components, strong mercury adsorption and oxidation ability, significant denitration effect, and good Hg 0 Oxidation rate, suitable for denitrification and demercuration emission control of fixed source flue gas such as thermal power plants, coking plants, waste incinerators, steel sintering machines, cement kilns, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0050] Figure 1 The oxidation rates of elemental Hg in flue gas by the catalysts prepared in Examples 1-4 of the present invention and Comparative Examples 1-2 are shown.

[0051] Figure 2 The denitration efficiency of the catalysts prepared in Examples 1-4 of the present invention and Comparative Examples 1-2;

[0052] Figure 3 This is a physical picture of the SCR honeycomb catalyst for denitrification and synergistic mercury removal prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0053] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0054] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0055] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0056] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0057] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0058] The raw material types and mass proportions of the SCR honeycomb catalyst for denitration and mercury removal in the embodiment of the present invention are shown in Table 1:

[0059] Table 1

[0060] name Mass fraction name Mass fraction Anatase Titanium Dioxide 63.5-65 Copper nitrate 1.9-2.2 Pseudoboehmite 1.0-1.2 Antimony acetate 1.3-1.6 Ammonium metavanadate-monoethanolamine aqueous solution 11-13 Silica Sol 1.5-2.5 Ammonium heptamolybdate 2.0-2.3 lactic acid 0.4-0.8 Ammonium Metatungstate 1.3-1.6 ammonia 3.5-5 Fiberglass 5-5.5 Sesbania powder 0.5-1 Cerium nitrate 1.1-1.5 Polyoxyethylene 0.5-1

[0061] The ammonium metavanadate-monoethanolamine aqueous solution is a homogeneous solution obtained by stirring and mixing ammonium metavanadate, monoethanolamine and water at a mass ratio of 1:1:3 at 75°C±5°C; the glass fiber is 6mm glass fiber; the silica sol is a 25% silica sol solution; the viscosity of the polyethylene oxide is 250mpa.s; the specific surface area of ​​the anatase titanium dioxide is 100m 2 / g, particle size distribution D50 is 1.2μm; pseudo-boehmite Al 2 O 3 ·nH 2 O (n = 0.55); the viscosity of sesbania powder is 850 mpa.s; the concentration of ammonia water is 25-27%; and the glass fiber is alkali-free glass fiber.

[0062] The composition of the raw materials by weight of Examples 1-4 and Comparative Examples 1-2 is shown in Table 2:

[0063] Table 2

[0064]

[0065] During the preparation process, the mass fraction of anatase titanium dioxide is used as the initial standard, and the remaining raw materials are weighed in sequence according to the proportion.

[0066] The preparation process of the SCR honeycomb catalyst for denitration and synergistic mercury removal in Example 1-4 is as follows:

[0067] (1) adding anatase titanium dioxide, silica sol, and pseudo-boehmite into a mixer and kneading them uniformly, adding deionized water until the water content is 38%, and mixing and stirring the obtained slurry mixture at 60° C. to obtain a mixture A;

[0068] (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to mixture A and mixing them uniformly to obtain mixture B;

[0069] (3) adding ammonia water to the obtained mixture B to adjust the pH value of the reaction system to 8.2, adding ammonium heptamolybdate and mixing evenly, then adding ammonium metavanadate-monoethanolamine aqueous solution, stirring for 60 minutes, and then heating and dehumidifying until the moisture content of the slurry in the mixer is 34%, thereby obtaining a mixture C;

[0070] (4) The mixture C was heated and stirred for 40 minutes to adjust the water content of the system to 30%, and then lactic acid was added to adjust the pH value to 7.6. Glass fiber was added and mixed. After that, sesbania powder and polyoxyethylene were added to adjust the water content of the system to 28%. After that, the mixture was aged to obtain aged mud D.

[0071] (5) The aged mud material D is extruded into strip-shaped mud material through a pre-extruder, and after removing impurities in the mud material, the honeycomb catalyst monomer is extruded through an extrusion die (30 holes).

[0072] (6) The extruded honeycomb catalyst monomer is dried in two stages and then calcined at a temperature of 500° C. for 35 h to obtain a denitrification and synergistic demercuration SCR honeycomb catalyst.

[0073] Among them, the two-stage drying is as follows:

[0074] First stage drying: first drying at 80% humidity and 40°C for 2 days, then drying at 60% humidity and 45°C for 4 days, and finally drying at 20% humidity and 55°C for 2 days. Second stage drying temperature is 60°C and time is 24h.

[0075] The actual picture of the denitration and mercury removal SCR honeycomb catalyst prepared in Example 1 of the present invention is shown in Figure 3 .

[0076] The preparation process of the catalyst of Comparative Example 1 is as follows:

[0077] (1) adding anatase titanium dioxide to a mixer and kneading the mixture uniformly, adding deionized water until the water content is 38%, and mixing the obtained slurry mixture uniformly at 60° C. to obtain a mixture A;

[0078] (2) adding ammonia water to the obtained mixture A to adjust the pH of the reaction system to 8.2, adding ammonium heptamolybdate and mixing evenly, then adding an ammonium metavanadate-monoethanolamine aqueous solution, stirring for 60 minutes, and then heating and dehumidifying until the moisture content of the slurry in the mixer is 34%, thereby obtaining a mixture B;

[0079] (3) The mixture B was heated and stirred for 40 minutes. When the water content of the system was 30%, lactic acid was added to adjust the pH value to 7.6. Glass fiber was then added and kneaded for 40 minutes to adjust the moisture content of the mud to 30%. Then, sesbania powder and polyoxyethylene were added and stirred continuously until the moisture content of the mixture was 28% and the pH value was 7.6. The mixture was then aged in the mixer for 8 hours to obtain aged mud C.

[0080] (4) The aged mud C is extruded into strip-shaped mud by a pre-extruder, and after removing impurities in the mud, the honeycomb catalyst monomer is extruded by an extrusion die (30 holes).

[0081] (5) The extruded honeycomb catalyst monomer was calcined after two-stage drying (two-stage drying was the same as in Example 1) at a calcination temperature of 500° C. and a calcination time of 35 h to obtain a catalyst.

[0082] The preparation process of the catalyst of Comparative Example 2 is as follows:

[0083] (1) adding anatase titanium dioxide to a mixer and kneading the mixture uniformly, adding deionized water until the water content is 38%, and mixing the obtained slurry mixture uniformly at 60° C. to obtain a mixture A;

[0084] (2) adding ammonium metatungstate to mixture A to obtain mixture B;

[0085] (3) adding ammonia water to the obtained mixture B to adjust the pH of the reaction system to 8.2, then adding an ammonium metavanadate-monoethanolamine aqueous solution, stirring for 60 minutes, and then heating and dehumidifying until the moisture content of the slurry in the mixer is 34%, thereby obtaining a mixture C;

[0086] (4) The mixture C was heated and stirred for 40 minutes, and the water content of the system was adjusted to 30%. Lactic acid was added to adjust the pH value to 7.6, and then glass fiber was added. After mixing for 40 minutes, the moisture content of the mud was adjusted to 30%. Then, field sesbania powder and polyoxyethylene were added, and stirring was continued to adjust the moisture content of the mixture to 28% and the pH value to 7.6. Then, the mixture was aged in the mixer for 8 hours to obtain aged mud D.

[0087] (5) The aged mud material D is extruded into strip-shaped mud material through a pre-extruder, and after removing impurities in the mud material, the honeycomb catalyst monomer is extruded through an extrusion die (30 holes).

[0088] (6) The extruded honeycomb catalyst monomer was calcined after two-stage drying (two-stage drying was the same as in Example 1) at a calcination temperature of 500° C. and a calcination time of 35 h to obtain a catalyst.

[0089] The component contents of the catalysts prepared in Example 1 of the present invention and Comparative Examples 1-2 are shown in Table 3, wherein the component contents are characterized by XRF (X-ray fluorescence spectrometer).

[0090] Table 3

[0091] sample <![CDATA[TiO 2 ]]> <![CDATA[V 2 THE 5 ]]> <![CDATA[MoO 3 ]]> <![CDATA[Sb 2 THE 3 ]]> <![CDATA[CeO 2 ]]> <![CDATA[WO 3 ]]> CuO <![CDATA[SO 3 ]]> <![CDATA[Na 2 The]]> (%) (%) (%) (%) (%) (%) (%) (%) (%) Example 1 81.318 2.25 2.008 0.874 0.998 1.615 0.75 1.187 0.212 Comparative Example 1 83.503 2.13 2.209 / / / / 2.837 0.262 Comparative Example 2 84.563 2.23 / / / 1.716 / 2.076 0.259 sample MgO <![CDATA[Al 2 THE 3 ]]> <![CDATA[SiO 2 ]]> <![CDATA[P 2 THE 5 ]]> <![CDATA[K 2 The]]> CaO <![CDATA[Fe 2 THE 3 ]]> <![CDATA[ZrO 2 ]]> <![CDATA[Nb 2 THE 5 ]]> (%) (%) (%) (%) (%) (%) (%) (%) (%) Example 1 0.203 1.214 5.001 0.014 0.036 2.17 0.111 0.014 0.025 Comparative Example 1 0.161 0.909 5.781 0.015 0.053 1.996 0.102 0.013 0.029 Comparative Example 2 0.162 1.001 5.802 0.006 0.057 1.987 0.099 0.015 0.027

[0092] The specific surface area, pore volume and pore diameter of the catalysts prepared in Examples 1-4 of the present invention and Comparative Examples 1-2 are shown in Table 4.

[0093] Table 4

[0094]

[0095] The radial compressive strength and axial compressive strength of the catalysts prepared in Examples 1-4 of the present invention and Comparative Examples 1-2 are shown in Table 5.

[0096] Table 5

[0097]

[0098] The catalysts prepared in Examples 1-4 and Comparative Examples 1-2 were placed in a 200-380°C, flue gas component NO (400 mg / Nm 3 ), O 2 (5%), ammonia nitrogen molar ratio is 1, SO 2 (400mg / Nm 3 )、Hg(450ng / m 3 ), carrier gas is N 2 , reaction space velocity is 4000h -1 The denitrification efficiency and elemental Hg oxidation rate were measured in a flue gas environment.

[0099] The results of the determination of the oxidation rate of elemental Hg in flue gas are shown in Table 6 and Figure 1 .

[0100] Table 6

[0101]

[0102]

[0103] The results of the denitrification efficiency determination are shown in Table 7 and Figure 2 .

[0104] Table 7

[0105]

[0106] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A denitration and mercury removal SCR honeycomb catalyst, characterized in that: The invention comprises the following raw material components in parts by weight: 63.5-65 parts of anatase-type catalytic titanium dioxide, 1.0-1.2 parts of pseudo-boehmite, 11-13 parts of ammonium metavanadate-monoethanolamine aqueous solution, 2.0-2.3 parts of ammonium heptamolybdate, 1.3-1.6 parts of ammonium metatungstate, 5-5.5 parts of glass fiber, 1.1-1.5 parts of cerium nitrate, 1.9-2.2 parts of copper nitrate, 1.3-1.6 parts of antimony acetate, 1.5-2.5 parts of silica sol, 0.5-1 parts of sesbania powder and 0.5-1 parts of polyoxyethylene.

2. The denitration and mercury removal SCR honeycomb catalyst according to claim 1, characterized in that: The ammonium metavanadate-monoethanolamine aqueous solution is a homogeneous solution obtained by mixing ammonium metavanadate, monoethanolamine and water in a mass ratio of 1:1:3 at 75°C±5°C.

3. The denitration and mercury removal SCR honeycomb catalyst according to claim 1, characterized in that: The raw material components also include 3.5-5 parts by mass of ammonia water and 0.4-0.8 parts by mass of lactic acid.

4. The method for preparing the SCR honeycomb catalyst for denitration and synergistic mercury removal according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) mixing anatase titanium dioxide, silica sol, pseudo-boehmite and water so that the water content of the system is 38%-39%, and stirring and mixing at 60-80° C. to obtain a mixture A; (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to the obtained mixture A, and mixing to obtain a mixture B; (3) adjusting the pH value of the mixture B to 8.2-8.5, then adding ammonium heptamolybdate and ammonium metavanadate-monoethanolamine aqueous solution to adjust the water content of the system to 33%-34%, to obtain a mixture C; (4) The mixture C is heated and stirred, and the water content of the system is adjusted to 30-31%, and the pH value is adjusted to 7.6-8.0, and glass fiber is added and mixed and stirred, and then sesbania powder and polyoxyethylene are added to adjust the water content of the system to 26-29%, and then aged. The aged mud is extruded and formed, and then dried and calcined to obtain the denitrification and synergistic mercury removal SCR honeycomb catalyst.

5. The method for preparing the SCR honeycomb catalyst for denitration and synergistic mercury removal according to claim 3, characterized in that: The following steps are involved: (1) mixing anatase titanium dioxide, silica sol, pseudo-boehmite and water so that the water content of the system is 38%-39%, and stirring and mixing at 60-80° C. to obtain a mixture A; (2) adding ammonium metatungstate, cerium nitrate, copper nitrate and antimony acetate to the obtained mixture A, and mixing to obtain a mixture B; (3) adding aqueous ammonia to make the pH value of mixture B 8.2-8.5, then adding ammonium heptamolybdate and ammonium metavanadate-monoethanolamine aqueous solution to adjust the water content of the system to 33%-34%, to obtain mixture C; (4) The mixture C is heated and stirred, and the water content of the system is adjusted to 30-31%, and then lactic acid is added to adjust the pH value to 7.6-8.0, and then glass fiber is added and mixed and stirred, and then sesbania powder and polyoxyethylene are added to adjust the water content of the system to 26-29%, and then aged. The aged mud is extruded into a shape, dried, and then calcined to obtain the denitrification and synergistic mercury removal SCR honeycomb catalyst.

6. Use of the denitration and synergistic mercury removal SCR honeycomb catalyst according to any one of claims 1 to 3 in flue gas denitration and / or mercury removal.

Citation Information

Patent Citations

  • Flue gas denitration catalyst applied at a low temperature and preparation method thereof

    CN105148904A

  • Medium and low temperature denitration catalyst and preparation method thereof

    CN106492791A

  • Wear-proof denitrification catalyst applicable to high-ash high-calcium work condition and preparation method thereof

    CN107552041A

  • High-low temperature denitration catalyst and preparation method thereof

    CN110773211A

  • Thallium poisoning resistant denitration catalyst, preparation method, application and application method

    CN112973720A

Cited By

  • SCR (Selective Catalytic Reduction) denitration catalyst as well as preparation method and application thereof

    CN119926429A

  • Sulfur-poisoning-resistant denitration and carbon monoxide-removing synergistic SCR (Selective Catalytic Reduction) catalyst and preparation method thereof

    CN120733755A

  • Preparation method and application of thallium-resistant SCR denitration catalyst for cement kiln