Sulfur-indium-zinc containing sulfur defect and tungsten oxide compounded S-type heterojunction photocatalyst as well as preparation method and application of sulfur-indium-zinc containing sulfur defect and tungsten oxide compounded S-type heterojunction photocatalyst

By constructing a sulfur-containing defective sulfur-indium zinc and tungsten oxide composite S-type heterojunction photocatalyst WO3/VS-Zn3In2S6, the problem of insufficient photocatalyst activity was solved, CO2 reduction activity and CH4 selectivity were significantly improved, and efficient Photocatalytic CO2 reduction reaction.

CN118807785AActive Publication Date: 2024-10-22FUZHOU UNIV

Patent Information

Application Number
CN202410993154.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-22
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing photocatalysts have insufficient activity in the CO2 reduction reaction, especially the photogenerated carrier recombination and insufficient active sites of zinc indium sulfide (Zn3In2S6) materials, which limits their catalytic activity.

Method used

The S-type heterojunction photocatalyst WO3/VS-Zn3In2S6, which contains sulfur-containing defective sulfur-indium zinc and tungsten oxide, is used to modify the catalyst to improve CO2 reduction activity and CH4 selectivity by constructing an S-type heterojunction and introducing sulfur defects. .

Benefits of technology

The CO2 reduction activity and CH4 selectivity are significantly improved, the CO generation rate is increased to 13.68 μmol·g-1·h-1, and the CH4 selectivity is increased from 43% to 72%, showing good photocatalysis under normal temperature and pressure. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807785A_ABST
    Figure CN118807785A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfur-containing indium zinc sulfide and tungsten oxide compounded S-type heterojunction photocatalyst as well as a preparation method and application thereof. The S-type heterojunction photocatalyst WO3 / VS-Zn3In2S6 is prepared by preparing a WO3 nanosheet through a hydrothermal method, loading the WO3 nanosheet on the surface of Zn3In2S6 through a solvothermal method, and then introducing sulfur defects through a light treatment method to prepare the S-type heterojunction photocatalyst WO3 / VS-Zn3In2S6. The S-type heterojunction photocatalyst WO3 / VS-Zn3In2S6 obtained by the invention has the characteristics of excellent activity, enhanced CH4 selectivity and good stability in the photocatalytic CO2 reduction reaction process, the preparation method is simple and feasible, and the S-type heterojunction photocatalyst WO3 / VS-Zn3In2S6 has a better application prospect in the photocatalytic CO2 reduction reaction process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of air treatment, energy conservation and emission reduction, and the preparation of high value-added chemical products using CO2, and specifically relates to an S-type heterojunction photocatalyst WO3 / V composite of sulfur-defective sulfur-indium zinc and tungsten oxide. S -Zn3In2S6 and its preparation method and application in photocatalytic CO2 reduction reaction. S -Zn3In2S6 catalyst can realize photocatalytic CO2 reduction to CO and CH4, and has good activity and stability, providing a new idea for photocatalytic CO2 reduction. Background Art

[0002] Nowadays, the concentration of carbon dioxide in the atmosphere has been rising year by year due to the massive consumption of fossil fuels, which has led to a series of environmental problems, including global warming, sea level rise, ocean acidification, extreme weather, species extinction and food shortage. So far, many methods have been explored to convert carbon dioxide, including thermal catalysis, electrocatalysis and photocatalysis. Thermal catalysis usually shows high efficiency for carbon dioxide reduction, but usually requires harsh conditions of high temperature and high pressure, resulting in considerable energy cost and safety issues. Electrocatalysis is carried out under an external electric field, and there is a trade-off between catalytic activity and selectivity due to the overpotential. In contrast, photocatalytic technology relies on solar energy to reduce carbon dioxide, showing advantages such as mild operating conditions, low energy consumption and ready availability. Inspired by artificial photosynthesis, photocatalytic reduction of CO2 using abundant solar energy, cost-effective water and photocatalysts can convert CO2 into organic matter, thereby alleviating the greenhouse effect and the imminent energy crisis.

[0003] At present, the photocatalytic carbon dioxide reduction on semiconductor photocatalysts has at least three main steps: 1. When the energy of the semiconductor photocatalyst is equal to or greater than the band gap energy (E g ) when irradiated by an appropriate light source, electron-hole pairs are generated. 2. The generated electrons and holes migrate to the surface of the semiconductor or the co-catalyst in contact with the semiconductor. It should be mentioned that only a part of the carrier can reach the surface of the semiconductor or the co-catalyst. A large part of the electron-hole pairs recombine together, and the energy is released in the form of heat or photons. 3. The photogenerated electrons reduce the CO2 adsorbed on the catalyst surface to CO, HCOOH, CH3OH or CH4, while the holes oxidize H2O to O2.

[0004] In recent years, among many semiconductor catalysts, zinc indium sulfide (Zn3In2S6) is one of the most promising photocatalysts because of its suitable conduction band and valence band positions for reducing and oxidizing CO2 and H2O, high light absorption efficiency, good chemical stability and other remarkable properties. It has been reported that it has shown catalytic activity in the photocatalytic reduction of CO2. However, the severe recombination of its photogenerated carriers and the lack of active sites limit the activity of this material in the photocatalytic reduction of CO2.

[0005] The S-type heterojunction is composed of an oxidized semiconductor OP and a reduced semiconductor RP. When they are in contact, the electrons in the RP with a higher Fermi level tend to transfer to the OP with a lower Fermi level, and the Fermi level reaches equilibrium, and the OP and RP form downward and upward band bends, respectively. At this time, RP is positively charged and OP is negatively charged, forming a built-in electric field from RP to OP. When illuminated, the electrons in OP and RP are excited from the valence band to the conduction band. Due to the effects of Coulomb attraction, built-in electric field and band bending, the photogenerated electrons in OP recombine with the photogenerated holes in RP, and the transfer of the photogenerated electrons in RP and the holes in OP is prevented, thereby retaining the photogenerated carriers with higher redox ability. The S-type heterojunction is feasible both in terms of charge transfer and redox ability improvement. However, the S-type heterojunction photocatalyst still cannot avoid the phenomenon of insufficient CO2 active sites. In the face of the above problems, the present invention uses a catalyst modification method to modify the catalyst by constructing an S-type heterojunction and introducing defects under light to achieve synergistic enhancement of CO2 reduction activity. Summary of the invention

[0006] In view of the problem that the catalyst activity in the existing photocatalytic CO2 reduction reaction is not high enough, the present invention provides an S-type heterojunction photocatalyst WO3 / V composite of sulfur-indium zinc and tungsten oxide containing sulfur defects. S -Zn3In2S6 and its preparation method and application, the method is simple and fast, and the prepared WO3 / V S -Zn3In2S6 catalyst has high photocatalytic reduction activity of CO2 and CH4 selectivity, which provides a new idea for the subsequent catalyst design and has good application prospects.

[0007] To achieve the above object, the present invention adopts the following technical solution: The invention discloses an S-type heterojunction photocatalyst composed of sulfur-defective indium zinc and tungsten oxide. The S-type heterojunction photocatalyst is an S-type heterojunction composite photocatalyst composed of sulfur-defective indium zinc as a reducing semiconductor and tungsten oxide as an oxidizing semiconductor.

[0008] Furthermore, the S-type heterojunction composite photocatalyst is WO3 / V S -Zn3In2S6, where WO3 and VS -The molar ratio of Zn3In2S6 is 10~40:100.

[0009] Furthermore, the S-type heterojunction composite photocatalyst was used to evaluate the carbon dioxide photoreduction activity in H2O vapor at room temperature and pressure using a 300W xenon lamp with a wavelength (λ) of 380 nm to 780 nm. The CO generation rate was 13.68 μmol·g under the conditions of high-purity CO2 and 3 mL of H2O in a gas-solid intermittent reactor. -1 ·h -1 The generation rate of CH4 is 34.68 μmol·g -1 ·h -1 , CH4 selectivity increased from 43% to 72%.

[0010] The above-mentioned method for preparing an S-type heterojunction photocatalyst comprises the following steps: preparing WO3 nanosheets using nitric acid solution and hydrated sodium tungstate as raw materials; adding hydrated zinc sulfate, hydrated indium nitrate and thioacetamide as raw materials, and hydrothermally synthesizing WO3 / Zn3In2S6 composite photocatalyst; introducing sulfur defects into the WO3 / Zn3In2S6 composite photocatalyst by light treatment method, and obtaining an S-type heterojunction photocatalyst WO3 / V S -Zn3In2S6 (abbreviated as WO3 / V S -ZIS).

[0011] The above-mentioned method for preparing an S-type heterojunction photocatalyst specifically comprises the following steps: S1: HNO3 was mixed with deionized water and stirred for 10 min to obtain solution A; Na2WO4·2H2O was dissolved in deionized water and stirred for 10 min to obtain solution B; solution A was dropped into solution B under magnetic stirring, and then stirred vigorously for 0.5 h, and the mixture was transferred to a hydrothermal device, sealed and reacted at 180℃ for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water, and then dried at 60℃ for 12 h to obtain WO3 nanosheets; S2: ZnSO4·7H2O and In(NO3)3·4.5H2O were dissolved in deionized water and stirred for 0.5 h, then CH3CSNH2 and WO3 nanosheets were added and stirred for another 0.5 h, the mixture was transferred to a hydrothermal device, sealed and reacted at 160 °C for 12 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water, and then dried at 60 °C for 12 h to obtain WO3 / Zn3In2S6 photocatalyst; S3: The WO3 / Zn3In2S6 photocatalyst was illuminated for 0.5 h to obtain the S-type heterojunction photocatalyst WO3 / V S-Zn3In2S6.

[0012] Furthermore, in the above step S1, the concentration of the HNO3 solution is 65%, and the amount used is 10 ml; the amount of Na2WO4·2H2O used is 1.0 g.

[0013] Furthermore, in the above step S2, the molar ratio of ZnSO4·7H2O, In(NO3)3·4.5H2O, CH3CSNH2, and WO3 nanosheets is 30:20:60:1~4.

[0014] Furthermore, in the above step S3, the illumination condition is as follows: the light source is a xenon lamp in the light wave band range of 380-780 nm, and the power of the xenon lamp is 300 W.

[0015] The above-mentioned S-type heterojunction photocatalyst is used in photocatalytic CO2 reduction.

[0016] The significant advantages of the present invention are: The present invention constructs an S-type heterojunction with a suitable proportion of WO3 nanosheets and introduces sulfur vacancies to modify Zn3In2S6 to obtain a WO3 / V S The sulfur vacancies on the surface of Zn3In2S6 catalyst act as adsorption sites for CO2, promoting the adsorption and activation of CO2. The S-type heterostructure assembled with WO3 nanosheets not only accelerates the migration and separation of photoexcited charge carriers, but also enhances the adsorption of H2O and V S The formation of S-type heterojunctions and sulfur vacancies in carbon dioxide reduction improves the activity and CH4 selectivity of the prepared catalyst in CO2 reduction reaction under UV-visible light. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 :V S -Zn3In2S6, WO3, 10% WO3 / V S -Zn3In2S6, 20%WO3 / V S -Zn3In2S6, 30%WO3 / V S -Zn3In2S6 and 40%WO3 / V S -XRD pattern of Zn3In2S6.

[0018] Figure 2 :V S -Zn3In2S6, WO3, 20% WO3 / V S -DRS pattern of Zn3In2S6.

[0019] Figure 3:V S -Zn3In2S6, WO3 and 20% WO3 / V S -SEM image of Zn3In2S6.

[0020] Figure 4 :V S -Zn3In2S6, WO3, 20% WO3 / V S -Photocurrent and impedance diagrams of Zn3In2S6.

[0021] Figure 5 :V S -Zn3In2S6, WO3, 10% WO3 / V S -Zn3In2S6, 20%WO3 / V S -Zn3In2S6, 30%WO3 / V S -Zn3In2S6 and 40%WO3 / V S -Evaluation diagram of the photocatalytic CO2 reduction activity and selectivity of Zn3In2S6. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the present invention clearer, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, not all embodiments. Based on the drawings and embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0023] Example 1: 10% WO3 / V S -Preparation of Zn3In2S6 S1: 10 mL of 65wt% HNO3 was mixed with 40 ml of deionized water and stirred for 10 min to obtain solution A; 1.0 g of Na2WO4·2H2O was dissolved in 20 ml of deionized water and stirred for 10 min to obtain solution B; the obtained solution A was dropped into solution B under magnetic stirring, and then vigorously stirred for 0.5 h, and the mixture was transferred to a hydrothermal device, sealed and reacted at 180℃ for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in sequence, and then dried at 60℃ for 12 h to obtain WO3 nanosheets (abbreviated as WO3).

[0024] S2: 3.0 mmol of ZnSO4·7H2O and 2.0 mmol of In(NO3)3·4.5H2O were dissolved in 60 ml of deionized water and stirred for 0.5 h. Subsequently, 6.0 mmol of CH3CSNH2 and 0.1 mmol of WO3 nanosheets were added and stirred for another 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in turn, and then dried at 60°C for 12 h to obtain a 10% WO3 / Zn3In2S6 photocatalyst.

[0025] S3: The WO3 / Zn3In2S6 photocatalyst was irradiated with a 300 W xenon lamp equipped with an infrared filter (wavelength range 380 nm-780 nm) for 0.5 h to obtain an S-type heterojunction photocatalyst 10% WO3 / V S -Zn3In2S6.

[0026] Example 2: 20% WO3 / V S -Preparation of Zn3In2S6 S1: 10 mL of 65wt% HNO3 was mixed with 40 ml of deionized water and stirred for 10 min to obtain solution A; 1.0 g of Na2WO4·2H2O was dissolved in 20 ml of deionized water and stirred for 10 min to obtain solution B; solution A was dropped into solution B under magnetic stirring, and then stirred vigorously for 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 180℃ for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in sequence, and then dried at 60℃ for 12 h to obtain WO3 nanosheets.

[0027] S2: 3.0 mmol of ZnSO4·7H2O and 2.0 mmol of In(NO3)3·4.5H2O were dissolved in 60 ml of deionized water and stirred for 0.5 h. Subsequently, 6.0 mmol of CH3CSNH2 and 0.2 mmol of WO3 nanosheets were added and stirred for another 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in turn, and then dried at 60°C for 12 h to obtain a 20% WO3 / Zn3In2S6 photocatalyst.

[0028] S3: The WO3 / Zn3In2S6 photocatalyst was irradiated with a 300 W xenon lamp equipped with an infrared filter (wavelength range 380 nm-780 nm) for 0.5 h to obtain an S-type heterojunction photocatalyst 20% WO3 / V S -Zn3In2S6.

[0029] Example 3: 30% WO3 / V S -Preparation of Zn3In2S6 S1: 10 mL of 65wt% HNO3 was mixed with 40 ml of deionized water and stirred for 10 min to obtain solution A; 1.0 g of Na2WO4·2H2O was dissolved in 20 ml of deionized water and stirred for 10 min to obtain solution B; solution A was dropped into solution B under magnetic stirring, and then stirred vigorously for 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 180℃ for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in sequence, and then dried at 60℃ for 12 h to obtain WO3 nanosheets.

[0030] S2: 3.0 mmol of ZnSO4·7H2O and 2.0 mmol of In(NO3)3·4.5H2O were dissolved in 60 ml of deionized water and stirred for 0.5 h. Subsequently, 6.0 mmol of CH3CSNH2 and 0.3 mmol of WO3 nanosheets were added and stirred for another 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in turn, and then dried at 60°C for 12 h to obtain a 30% WO3 / Zn3In2S6 photocatalyst.

[0031] S3: The WO3 / Zn3In2S6 photocatalyst was irradiated with a 300 W xenon lamp equipped with an infrared filter (wavelength range 380 nm-780 nm) for 0.5 h to obtain an S-type heterojunction photocatalyst 30% WO3 / V S -Zn3In2S6.

[0032] Example 4: 40% WO3 / V S -Preparation of Zn3In2S6 S1: 10 mL of 65wt% HNO3 was mixed with 40 ml of deionized water and stirred for 10 min to obtain solution A; 1.0 g of Na2WO4·2H2O was dissolved in 20 ml of deionized water and stirred for 10 min to obtain solution B; solution A was dropped into solution B under magnetic stirring, and then stirred vigorously for 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 180℃ for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in sequence, and then dried at 60℃ for 12 h to obtain WO3 nanosheets.

[0033] S2: 3.0 mmol of ZnSO4·7H2O and 2.0 mmol of In(NO3)3·4.5H2O were dissolved in 60 ml of deionized water and stirred for 0.5 h. Subsequently, 6.0 mmol of CH3CSNH2 and 0.4 mmol of WO3 nanosheets were added and stirred for another 0.5 h. The mixture was transferred to a hydrothermal device, sealed and reacted at 160°C for 12 h. After the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in turn, and then dried at 60°C for 12 h to obtain a 40% WO3 / Zn3In2S6 photocatalyst.

[0034] S3: The WO3 / Zn3In2S6 photocatalyst was illuminated using a 300 W xenon lamp equipped with an infrared filter (light waveband range 380 nm-780 nm) for 0.5 h to obtain an S-type heterojunction photocatalyst 40% WO3 / V S -Zn3In2S6.

[0035] Comparative Example: S1: 3.0 mmol of ZnSO4·7H2O and 2.0 mmol of In(NO3)3·4.5H2O were dissolved in 60 ml of deionized water and stirred for 0.5 h, then 6.0 mmol of CH3CSNH2 was added and stirred for another 0.5 h, the mixture was transferred to a hydrothermal apparatus, sealed and reacted at 160°C for 12 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water in turn, and then dried at 60°C for 12 h to obtain Zn3In2S6 photocatalyst.

[0036] S2: The Zn3In2S6 photocatalyst was irradiated with a 300 W xenon lamp equipped with an infrared filter (light waveband range 380 nm-780 nm) for 0.5 h to obtain the sulfur vacancy Zn3In2S6 photocatalyst V S -Zn3In2S6 (abbreviated as V S -ZIS).

[0037] Catalyst performance evaluation: The photoreduction activity of CO2 in H2O vapor was evaluated in a 175 mL gas-solid batch reactor. 20 mg of the photocatalyst was dispersed in 3 mL of water, spread on a tray, and then dried at 80 °C to form a uniform film before being placed in the reactor. Subsequently, the reactor was evacuated with a vacuum pump and injected with CO2 (99.999%). Then, 2 mL of deionized water was injected into the bottom of the reactor and stirred continuously with a magnetic stirrer. After that, a 300 W Xe lamp equipped with an infrared filter (light waveband range 380 nm to 780 nm) was placed 2–3 cm above the top of the reactor. After the specified reaction time interval, 1 mL of the reaction gas was extracted from the reactor with a chromatographic needle for analysis. The gaseous products were analyzed using a gas chromatograph (Agilent 7890B) equipped with a highly sensitive thermal conductivity detector (TCD) and a flame ionization detector (FID).

[0038] The gas yield can be calculated by the following formula: Where Y is the gas yield, k is the standard curve coefficient of the gas measured by the external standard method, S a is the area for gas chromatography to measure gas content, V is the reactor volume, m cat is the mass of catalyst and t is the reaction time.

[0039] The performance of photocatalytic CO2 reduction of various catalysts was evaluated according to this method, and the results are shown in Table 1: Table 1 Catalytic CO2 reduction performance of different catalysts

[0040] As shown in Table 1, the introduction of sulfur defects significantly increased V compared to Zn3In2S6 catalyst. S -The activity of Zn3In2S6, after compounding with WO3, WO3 / V S -Zn3In2S6 photocatalytic CO2 reduction activity was further significantly enhanced, and CH4 selectivity was improved.

[0041] Figure 1 V S -Zn3In2S6, WO3, 10% WO3 / V S -Zn3In2S6, 20%WO3 / V S -Zn3In2S6, 30%WO3 / V S -Zn3In2S6 and 40%WO3 / V S -XRD pattern of Zn3In2S6. Figure 1 It can be seen that in WO3 / V SPeaks belonging to WO3 and ZIS were observed in the ZIS-WO composites, and the intensity of the WO3 diffraction peak increased slightly with the increase of WO3 content in the composites. At the same time, no other impurities were detected, reflecting that the prepared samples had good phase purity.

[0042] Figure 2 V S -Zn3In2S6, WO3 and 20%WO3 / V S -DRS image of Zn3In2S6. Figure 2 It can be seen that V S -The maximum absorption edges of Zn3In2S6 and WO3 are approximately 500 nm and 460 nm, respectively, indicating that both are photocatalysts responsive to visible light.

[0043] Figure 3 V S -Zn3In2S6, WO3 and 20%WO3 / V S -SEM image of Zn3In2S6. Figure 3 It can be seen that V S -Zn3In2S6 shows a flower-shaped microsphere structure composed of ultrathin, smooth, interlaced two-dimensional nanosheets. Figure 3 b It can be seen that WO3 is composed of irregular two-dimensional nanosheets. Figure 3 cd shows that WO3 nanosheets are firmly embedded in V S -Zn3In2S6 microspheres, a 2D / 2D hybrid structure was formed.

[0044] Figure 4 V S -Zn3In2S6, WO3 and 20%WO3 / V S -Photocurrent and impedance diagram of Zn3In2S6. Larger photocurrent response and smaller impedance radius indicate better electron transfer ability, which will accelerate electron transfer and inhibit the recombination of photogenerated electron-hole pairs. From the photocurrent flow diagram ( Figure 4 a) It can be seen that the photocurrent response of WO3 is almost negligible, while 20% WO3 / V S -The photocurrent response of the Zn3In2S6 composite material significantly exceeds that of V alone S -Zn3In2S6, 20% WO3 / V S -Zn3In2S6 composite material has the highest photocurrent response. From the electrochemical impedance spectroscopy (EIS) ( Figure 4 b) The measurement results show that 20% WO3 / V S -The semicircle diameter of Zn3In2S6 composite materials is smaller than that of WO3 and V S-Semicircle diameter of Zn3In2S6. 20% WO3 / V S -Zn3In2S6 has the smallest arc radius in the spectrum, indicating that it has the lowest electrochemical impedance. This indicates that due to the construction of the S-type heterojunction, 20%WO3 / V S -Zn3In2S6 can generate more photogenerated electrons under ultraviolet and visible light irradiation, and the resistance to the transfer of photogenerated electrons will be smaller, which is conducive to more photogenerated electrons participating in the reaction, thereby improving the performance of the catalyst.

[0045] Figure 5 V S -Zn3In2S6, WO3, 10% WO3 / V S -Zn3In2S6, 20%WO3 / V S -Zn3In2S6, 30%WO3 / V S -Zn3In2S6 and 40%WO3 / V S -Evaluation diagram of the photocatalytic CO2 reduction activity and selectivity of Zn3In2S6. Figure 5 It can be seen that at room temperature and pressure, a 300W xenon lamp was used to control the wavelength (λ) range of 380 nm - 780 nm to evaluate the CO2 photoreduction activity in H2O vapor. A gas-solid intermittent reactor was used to introduce high-purity CO2 and 3 mL of H2O. S -Zn3In2S6 catalyst has the best activity and CH4 selectivity, and the CO generation rate is 13.68 μmol·g -1 ·h -1 The generation rate of CH4 is 34.68 μmol·g -1 ·h -1 , CH4 selectivity increased from 43% to 72%. In terms of the working principle, when the WO3 loading is less than 20%, the newly added adsorption activation sites on the surface of the material are not enough, making the activity not good enough; when the content is higher than 20%, excessive WO3 loading reduces the adsorption activation sites due to aggregation and shielding, which will lead to a decrease in activity.

[0046] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. An S-type heterojunction photocatalyst composed of sulfur-deficient indium zinc and tungsten oxide, Features: The S-type heterojunction photocatalyst is an S-type heterojunction composite photocatalyst which is compositely constructed by using sulfur-defective indium zinc as a reduction semiconductor and tungsten oxide as an oxidation semiconductor.

2. The S-type heterojunction photocatalyst according to claim 1, Features: The S-type heterojunction composite photocatalyst is WO 3 / V S -Zn 3 In 2 S 6 , where WO 3 With V S -Zn 3 In 2 S 6 The molar ratio is 10~40:

100.

3. The method for preparing the S-type heterojunction photocatalyst according to any one of claims 1 to 2, Features: Preparation of WO using nitric acid solution and hydrated sodium tungstate as raw materials 3 Nanosheets; using hydrated zinc sulfate, hydrated indium nitrate and thioacetamide as raw materials, adding WO 3 Nanosheets, hydrothermal synthesis of WO 3 / Zn 3 In 2 S 6 Composite photocatalyst; Photocatalytic treatment of WO 3 / Zn 3 In 2 S 6 Sulfur defects were introduced into the composite photocatalyst to obtain the S-type heterojunction photocatalyst WO 3 / V S -Zn 3 In 2 S 6 .

4. The preparation method according to claim 3, Features: The specific steps include: S1: HNO 3 The solution was mixed with deionized water and stirred for 10 min to obtain solution A. 2 WO 4 ·2H 2 O was dissolved in deionized water and stirred for 10 min to obtain solution B; solution A was dropped into solution B under magnetic stirring, and then stirred vigorously for 0.5 h. The mixed solution was transferred to a hydrothermal device, sealed and reacted at 180 °C for 3 h; after the reaction was completed, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water, and then dried at 60 °C for 12 h to obtain WO 3 Nanosheets; S2: Place ZnSO 4 7H 2 O and In(NO 3 ) 3 4.5H 2 O was dissolved in deionized water and stirred for 0.5 h, followed by addition of CH 3 CSNH 2 and WO 3 The mixture was transferred to a hydrothermal device, sealed and reacted at 160 °C for 12 h. After the reaction, it was cooled to room temperature, the precipitate was collected by centrifugation and washed with ethanol and deionized water, and then dried at 60 °C for 12 h to obtain WO 3 / Zn 3 In 2 S 6 Photocatalysts; S3: to WO 3 / Zn 3 In 2 S 6 The photocatalyst was illuminated for 0.5 h to obtain the S-type heterojunction photocatalyst WO 3 / V S -Zn 3 In 2 S 6 .

5. The preparation method according to claim 4, Features: In step S1, HNO 3 The concentration of the solution is 65%, the dosage is 10 ml; Na 2 WO 4 ·2H 2 The amount of O used was 1.0 g.

6. The preparation method according to claim 4, Features: In step S2, ZnSO 4 7H 2 O、In(NO 3 ) 3 4.5H 2 O、CH 3 CSNH 2 , WO 3 The molar ratio of the nanosheets is 30:20:60:1~4.

7. The preparation method according to claim 4, Features: In step S3, the illumination conditions are as follows: the light source is a xenon lamp in the light wave band range of 380-780 nm, and the power of the xenon lamp is 300 W.

8. The S-type heterojunction photocatalyst according to any one of claims 1 to 2 is used for photocatalytic CO 2 Restore application.

Citation Information

Patent Citations

  • Preparation and application of Z-shaped structure hybrid titanium dioxide photocatalyst

    CN108404934A

  • Preparation method of WO3 / Ag: ZnIn2S4 composite semiconductor photocatalyst

    CN113134364A

  • Bacillus velezensis PGR-1 and uses thereof

    KR1020250058203A

Cited By

  • Sulfur defect heterojunction molybdenum disulfide and light induction preparation method and application thereof

    CN119710783A

  • A sulfur-defect heterojunction molybdenum disulfide and a light-induced preparation method and application thereof

    CN119710783B

  • S-type WO3 / FeWO4 heterojunction photocatalyst as well as synthesis method and application method thereof

    CN119926417A

  • Porous photo-thermal catalyst based on reverse confinement induction as well as preparation and application of porous photo-thermal catalyst

    CN120827885A

  • Crystalline Cu-In-S / amorphous ZnWO4 double-vacancy heterojunction photocatalyst and preparation method thereof

    CN122517055A