Gold nanoparticles as well as preparation method and application thereof
By using gold nanoparticles prepared under ice-water bath conditions, the problems of drug resistance and adverse reactions of existing antibiotics in the treatment of bacterial infections have been solved, and efficient bacteriostasis and sterilization of Gram-positive bacteria have been achieved, with good biological properties. Compatibility and antimicrobial properties.
Patent Information
- Application Number
- CN202410777162.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing antibiotics have drug resistance problems and adverse reactions in the treatment of bacterial infections, and the resistance genes of superbugs can spread rapidly, resulting in reduced treatment effectiveness.
A method for preparing gold nanoparticles is adopted. By preparing a mixed solution of gold salt, ligand and stabilizer, and performing a reduction reaction under ice-water bath conditions, gold nanoparticles with good biocompatibility and antibacterial properties are obtained.
Gold nanoparticles have broad-spectrum antibacterial functions against Gram-positive bacteria, exhibit long-lasting antibacterial and efficient bactericidal properties, and have good biocompatibility, which can effectively control the infection and spread of drug-resistant bacteria.
Smart Images

Figure CN118808665A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomaterials, and in particular to a nano-gold particle and a preparation method and application thereof. Background Art
[0002] Bacteria, as pathogens, can invade host cells, produce pathogenic substances and cause host infection. According to statistics, 100,000 deaths are randomly selected from the number of deaths each year, of which about 33,000 deaths are directly caused by bacterial infections. Antibiotics are used to treat diseases related to bacterial infections to reduce the harm caused by bacterial infections. However, although antibiotics are very successful in treating bacterial infections, with the abuse of antibiotics, this has not only caused a large amount of waste of medical supplies, but also the related problems of drug resistance and adverse reactions have become increasingly prominent. In addition, because the resistance genes of super bacteria can spread rapidly between different bacteria, antibiotics previously used to treat bacterial infections are also facing the problem of ineffectiveness.
[0003] Therefore, it is important to provide new antibacterial substances. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing nano-gold particles, which has a simple process and can prepare nano-gold particles with good biocompatibility and antibacterial properties.
[0005] The invention also provides nano gold particles prepared by the preparation method.
[0006] The present invention also provides an antibacterial composition comprising nano-gold particles.
[0007] The present invention also provides the application of the preparation method or the nano-gold particles or the antibacterial composition.
[0008] A method for preparing gold nanoparticles according to a first aspect of the present invention comprises the following steps:
[0009] A first mixed solution of a gold salt, a ligand and a stabilizer is prepared, and a first reaction is carried out to obtain a reaction solution; a second mixed solution containing a reducing agent and the reaction solution is prepared, and a second reaction is carried out to obtain nano-gold particles;
[0010] The ligand has a structure shown in the following general formula:
[0011]
[0012] R1 is selected from Cl, Br, C1-C4 alkane or hydroxyl;
[0013] R2 is selected from Cl, Br, C1-C4 alkane or hydroxyl.
[0014] According to some embodiments of the present invention, the reaction temperature of the preparation method is 0-4°C.
[0015] According to some embodiments of the present invention, the C1-C4 alkane group is -CH3, -CH2CH3, -CH2CH2CH3 or -CH2CH2CH2CH3.
[0016] According to some embodiments of the present invention, the gold salt is a soluble gold salt, and the gold salt includes at least one of chloroauric acid, tetrachloroauric acid trihydrate, and tetrachloroauric acid tetrahydrate.
[0017] According to some embodiments of the present invention, the stabilizer includes at least one of thiol PEG, Tween 80, and PVP. The stabilizer can make the synthesized nano-gold particles more stable, otherwise the synthesized nano-gold particles will precipitate quickly in water.
[0018] According to some embodiments of the present invention, the number average molecular weight of the thiol PEG is 500 to 5000. Thus, the colloidal stability of the gold nanoparticles can be better ensured.
[0019] According to some embodiments of the present invention, the ligand includes at least one of the compounds represented by formula I, the compounds represented by formula II, the compounds represented by formula III, the compounds represented by formula IV, and the compounds represented by formula V.
[0020]
[0021] According to some embodiments of the present invention, the molar ratio of the gold salt to the ligand is 1:0.1 to 2.5, for example, 1:0.1, 1:0.2, 1:0.4, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4 or 1:2.5.
[0022] According to some embodiments of the present invention, the molar ratio of the ligand to the stabilizer is 1:0.005-0.25. For example, it can be 1:0.005, 1:0.01, 1:0.02, 1:0.04, 1:0.06, 1:0.08, 1:0.1, 1:0.12, 1:0.14, 1:0.16, 1:0.18, 1:0.2 or 1:0.25.
[0023] According to some embodiments of the present invention, when the ligand is a compound of formula I: the molar ratio of the gold salt to the ligand is 1:1.8-2.2, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22. The molar ratio of the gold salt to the ligand is 1:0.8-1.2, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22. The molar ratio of the gold salt to the ligand is 1:0.4-0.6, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22). The molar ratio of the gold salt to the ligand is 1:0.2-0.3, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22 or 1:0.18-0.22). The molar ratio of the gold salt to the ligand is 1:0.1-0.15, and the molar ratio of the ligand to the stabilizer is 1:0.18-0.22.
[0024] According to some embodiments of the present invention, when the ligand is a compound of formula II: the molar ratio of the gold salt to the ligand is 1:1.8-2.2, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.12). The molar ratio of the gold salt to the ligand is 1:0.8-1.2, and the molar ratio of the ligand to the stabilizer is 1:0.018-0.22 (for example, it can be 1:0.08-0.22). The molar ratio of the gold salt to the ligand is 1:0.4-0.6, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22 or 1:0.08-0.12). The molar ratio of the gold salt to the ligand is 1:0.1-0.15, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22 (for example, it can be 1:0.18-0.22).
[0025] According to some embodiments of the present invention, when the ligand is a compound represented by formula III: the molar ratio of the gold salt to the ligand is 1:1.8-2.2, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22. The molar ratio of the gold salt to the ligand is 1:0.8-1.2, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22.
[0026] According to some embodiments of the present invention, when the ligand is a compound represented by formula IV: the molar ratio of the gold salt to the ligand is 1:1.8-2.2, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22 (for example, it can be 1:0.18-0.22). The molar ratio of the gold salt to the ligand is 1:0.8-1.2, and the molar ratio of the ligand to the stabilizer is 1:0.08-0.22 (for example, it can be 1:0.08-0.12). The molar ratio of the gold salt to the ligand is 1:0.4-0.6, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22 or 1:0.18-0.22). The molar ratio of the gold salt to the ligand is 1:0.1-0.15, and the molar ratio of the ligand to the stabilizer is 1:0.18-0.22).
[0027] According to some embodiments of the present invention, when the ligand is a compound represented by formula V: the molar ratio of the gold salt to the ligand is 1:1.8-2.2, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22). The molar ratio of the gold salt to the ligand is 1:0.8-1.2, and the molar ratio of the ligand to the stabilizer is 1:0.03-0.22 (for example, it can be 1:0.08-0.22 or 1:0.18-0.22).
[0028] According to some embodiments of the present invention, the concentration of the gold salt in the first mixed solution is 30-50 mg / mL, for example, 30 mg / mL, 35 mg / mL, 40 mg / mL, 45 mg / mL or 50 mg / mL.
[0029] According to some embodiments of the present invention, the reaction solvent of the first reaction and / or the second reaction includes at least one of methanol and deionized water.
[0030] According to some embodiments of the present invention, the preparation of the first mixed solution of gold salt, ligand and stabilizer comprises: adding ligand solution and stabilizer solution dropwise to the gold salt solution. The volume ratio of the gold salt solution to the ligand solution and the stabilizer solution is 1:0.4-0.6:0.4-0.6.
[0031] According to some embodiments of the present invention, the reaction time of the first reaction is 10 to 30 minutes, for example, 10 minutes, 15 minutes, 20 minutes, 25 minutes or 30 minutes.
[0032] According to some embodiments of the present invention, the reducing agent includes sodium borohydride (NaBH4).
[0033] According to some embodiments of the present invention, the molar ratio of the gold salt to the reducing agent is 1:2 to 4. For example, it may be 1:2, 1:2.3, 1:2.5, 1:2.7, 1:3, 1:3.3, 1:3.5, 1:3.8 or 1:4.
[0034] According to some embodiments of the present invention, the concentration of the reducing agent in the second mixed solution is 0.3-0.6 mg / mL, for example, 0.3 mg / mL, 0.35 mg / mL, 0.4 mg / mL, 0.45 mg / mL, 0.5 mg / mL, 0.55 mg / mL or 0.6 mg / mL.
[0035] According to some embodiments of the present invention, preparing a second mixed solution containing a reducing agent and a reaction solution includes: dropping a reducing agent solution into the reaction solution. The concentration of the reducing agent solution is 2 to 3 mg / mL. For example, it can be 2 mg / mL, 2.1 mg / mL, 2.2 mg / mL, 2.3 mg / mL, 2.4 mg / mL, 2.5 mg / mL, 2.6 mg / mL, 2.7 mg / mL, 2.8 mg / mL, 2.9 mg / mL or 3 mg / mL. By dropping and stirring the reaction, the reducing agent can be more fully reduced to obtain nano-gold particles.
[0036] According to some embodiments of the present invention, the reaction time of the second reaction is 70 to 100 min, for example, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min or 100 min.
[0037] According to some embodiments of the present invention, the second reaction includes reacting for 10 to 20 minutes at a first speed and reacting for 50 to 80 minutes at a second speed; the first speed is greater than the second speed.
[0038] According to some embodiments of the present invention, the first rotation speed is 1000-2000 rpm, for example, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, 1500 rpm, 1600 rpm, 1700 rpm, 1800 rpm, 1900 rpm or 2000 rpm.
[0039] According to some embodiments of the present invention, the second rotation speed is 400 rpm to 800 rpm, for example, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm or 800 rpm.
[0040] According to some embodiments of the present invention, the preparation method further comprises post-reaction treatment, and the post-reaction treatment comprises purification treatment.
[0041] According to some embodiments of the present invention, the purification treatment comprises dialysis. The molecular weight cut-off of the dialysis is 12 to 15 kDa (for example, 14 kDa). The dialysis time is 48 to 72 hours.
[0042] According to the second aspect of the present invention, the nano-gold particles are prepared by the above-mentioned preparation method.
[0043] According to some embodiments of the present invention, the average hydrated particle size of the nano-gold particles is 8 nm to 50 nm, for example, 8 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or 50 nm.
[0044] According to some embodiments of the present invention, the potential of the gold nanoparticles is -25mV to -5mV, for example, -25mV, -23mV, -20mV, -18mV, -15mV, -13mV, -10mV, -8mV or -5mV.
[0045] According to some embodiments of the present invention, the MIC value of the nano-gold particles against MRSA is 0.5-32 μg / mL.
[0046] An antibacterial composition according to a third aspect of the present invention comprises the nano-gold particles described in the second aspect of the present invention.
[0047] According to some embodiments of the present invention, the antibacterial composition may further include other components having antibacterial activity, preferably so as not to affect the effect of the nano-gold particles.
[0048] According to some embodiments of the present invention, the antibacterial composition further comprises an auxiliary material or a carrier.
[0049] According to the fourth aspect of the present invention, the preparation method as described in the first aspect embodiment above, the nanogold particles as described in the second aspect embodiment above, or the antibacterial composition as described in the third aspect embodiment above are used in the preparation of antibacterial products.
[0050] According to some embodiments of the present invention, the gold nanoparticles are used to inhibit bacterial cell wall synthesis.
[0051] According to some embodiments of the present invention, the antimicrobial product is selected from a drug, a preparation, a kit, a packaging material, a medical product or a fabric.
[0052] According to some embodiments of the present invention, the antimicrobial product is used to fight bacteria.
[0053] According to some embodiments of the present invention, the bacteria include Gram-positive bacteria. The Gram-positive bacteria include clinical isolates that are resistant to antibiotics.
[0054] According to some embodiments of the present invention, the Gram-positive bacteria include at least one of Staphylococcus aureus, methicillin-resistant Staphylococcus aureus, Staphylococcus epidermidis, methicillin-resistant Staphylococcus epidermidis, Enterococcus faecalis, multidrug-resistant Enterococcus faecalis, Staphylococcus haemolyticus, and methicillin-resistant Staphylococcus haemolyticus.
[0055] The present invention has at least the following beneficial effects:
[0056] The nano-gold particles of the present invention have a broad-spectrum antibacterial function to Gram-positive bacteria, show the characteristics of long-term antibacterial and efficient sterilization, and have better antibacterial performance than the currently commonly used antibiotic vancomycin in clinical practice. In addition, these antibacterial gold particles have good biocompatibility, are good candidate drugs for anti-Gram-positive bacterial infection, and are expected to be used to control bacterial infection and spread caused by Gram-positive bacteria. The preparation method of the present embodiment is prepared by a one-pot method, and the process is simple, and the prepared antibacterial material has excellent colloidal stability and excellent antibacterial performance. In short, the present invention helps to control the infection and spread of drug-resistant bacteria, is of great significance for improving people's quality of life and promoting social health, and has significant social, economic and technical benefits as well as very high practical application value and promotion prospects.
[0057] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 The MIC value test results of the nano-gold particles prepared by the compound shown in Formula I on different Staphylococcus aureus; wherein, Figure A is Staphylococcus aureus ATCC 29213, and Figure B is MRSA;
[0059] Figure 2 The MIC value test results of the gold nanoparticles prepared by the compound shown in Formula II against different Staphylococcus aureus; wherein, Figure A is Staphylococcus aureus ATCC 29213, and Figure B is MRSA;
[0060] Figure 3 The MIC value test results of the gold nanoparticles prepared from the compound represented by Formula III against different Staphylococcus aureus; wherein, Figure A is Staphylococcus aureus ATCC 29213, and Figure B is MRSA;
[0061] Figure 4The MIC value test results of the gold nanoparticles prepared from the compound represented by Formula IV against different Staphylococcus aureus; wherein, Figure A is Staphylococcus aureus ATCC 29213, and Figure B is MRSA;
[0062] Figure 5 The MIC value test results of the gold nanoparticles prepared from the compound of formula V on different Staphylococcus aureus; wherein, Figure A is Staphylococcus aureus ATCC 29213, and Figure B is MRSA;
[0063] Figure 6 The average particle size test results of the gold nanoparticles in Examples 1 and 2;
[0064] Figure 7 The potential value test results of the gold nanoparticles in Examples 1 and 2;
[0065] Figure 8 is the UV-visible absorption spectrum of the gold nanoparticles of Examples 1 and 2;
[0066] Fig. 9 The time-kill curves of the gold nanoparticles of low concentrations in Examples 1 and 2;
[0067] Fig.10 The time-kill curves of the gold nanoparticles of high concentrations in Examples 1 and 2;
[0068] Fig.11 The effect of the gold nanoparticles in Examples 1 and 2 on the growth curve of Staphylococcus aureus ATCC 29213; wherein, Figure A is the growth curve at a concentration of 1 μg / mL, and Figure B is the growth curve at a concentration of 2 μg / mL;
[0069] Fig.12 The effect of the gold nanoparticles in Examples 1 and 2 on the growth curve of MRSA; wherein, Figure A is the growth curve at a concentration of 1 μg / mL, and Figure B is the growth curve at a concentration of 2 μg / mL;
[0070] Fig.13 The effects of the gold nanoparticles in Examples 1 and 2 on the blood routine indexes of mice;
[0071] Fig.14 The effects of the gold nanoparticles in Examples 1 and 2 on the blood biochemical indices of mice;
[0072] Fig.15 This is a TEM photo of the effect of gold nanoparticles on bacteria in Example 2;
[0073] Fig.16 This is the in vivo antibacterial effect of the gold nanoparticles of Example 2. DETAILED DESCRIPTION
[0074] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0075] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0076] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0077] In the description of the present invention, the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.
[0078] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0079] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, or article that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, or article.
[0080] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0081] In the embodiments of the present invention, the number average molecular weight of the thiol PEG used is 2000, purchased from SIGMA-ALDRICH, with the product number 729140-1G and the trade name of polyethylene glycol methyl ether thiol.
[0082] In the embodiment of the present invention, the MIC value of the gold nanoparticles is detected by the following method. The steps are as follows:
[0083] 1) Preparation of bacterial culture solution: Staphylococcus aureus ATCC 29213 (Staphylococcus aureus, referred to as Sa in this application), MRSA, Staphylococcus epidermidis (referred to as SE in this application), methicillin-resistant Staphylococcus epidermidis (MRSE), Enterococcus faecalis (referred to as EF in this application), multidrug-resistant Enterococcus faecalis (MREF), Staphylococcus hemolyticus (referred to as SH in this application), and methicillin-resistant Staphylococcus hemolyticus (MRSH) were inoculated into LB solid culture plates, and cultured at 37° C. overnight; single colonies were continuously selected and inoculated into LB liquid culture medium, and cultured at 37° C. overnight; an appropriate amount of bacterial suspension was taken and diluted with LB liquid culture medium to a bacterial concentration of 10 6 CFU / mL to obtain the diluted bacterial suspension.
[0084] 2) Preparation of drug solution: Dilute the gold nanoparticles to a certain concentration using LB liquid culture medium to obtain a series of particle solutions with a concentration gradient.
[0085] 3) Perform MIC determination: Add equal volumes of diluted bacterial suspension and drug solution to a 96-well plate. Repeat 3 times for each treatment group. After incubation in a 37°C incubator for 24 hours, observe the colony growth and turbidity of each well to determine the lowest drug concentration that inhibits colony proliferation. Compared with the blank control group, from high concentration to low concentration, the lowest drug concentration that keeps the culture solution clear is the MIC.
[0086] Effect of the compound represented by formula Ⅰ (ligand 23) on the antibacterial properties of gold nanoparticles
[0087] The compound represented by formula Ⅰ (CAS number 51618-29-2) was used as a ligand to prepare gold nanoparticles, and the effect of synthesis conditions on the antibacterial properties of gold nanoparticles was investigated by the orthogonal method.
[0088]
[0089] The preparation of gold nanoparticles was carried out in an ice water bath. The specific steps are as follows:
[0090] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (dissolved in methanol) and 5mL of thiol PEG solution (dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in an ice-water bath for one hour. The reaction solution is dialyzed with deionized water (14kDa MW cut-toff, Millipore) for 72h and sterilized with a 0.22μm filter (Millipore) to obtain nanogold particles.
[0091] Wherein, different ligand addition amounts are set, and the ligand solution contains 0.2mmol, 0.1mmol, 0.05mmol, 0.025mmol, and 0.0125mmol of the compound represented by formula I, respectively, that is, the molar ratio of gold to ligand (Au:ligand) is 1:2, 1:1, 2:1, 4:1, and 8:1, respectively. Different thiol PEG addition amounts are set, so that the molar ratio of thiol PEG to ligand (PEG:ligand) is 0.01:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively, corresponding to 1%, 2%, 5%, 10%, and 20%, respectively; for example: when the ligand solution contains 0.2mmol of the compound represented by formula I, and the thiol PEG solution contains 0.04mmol of thiol PEG, then PEG:ligand is 20%.
[0092] The MIC value test results of gold nanoparticles are as follows Figure 1 shown.
[0093] Effect of the compound represented by formula II (ligand 34) on the antibacterial properties of gold nanoparticles
[0094] The compound represented by formula II (CAS number 5331-91-9) was used as a ligand to prepare gold nanoparticles, and the effect of synthesis conditions on the antibacterial properties of gold nanoparticles was investigated by the orthogonal method.
[0095]
[0096] The preparation of gold nanoparticles was carried out in an ice water bath. The specific steps are as follows:
[0097] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (dissolved in methanol) and 5mL of thiol PEG solution (dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in an ice-water bath for one hour. The reaction solution is dialyzed with deionized water (14kDa MW cut-toff, Millipore) for 72h and sterilized with a 0.22μm filter (Millipore) to obtain nanogold particles.
[0098] Wherein, different ligand addition amounts are set, and the ligand solution contains 0.2mmol, 0.1mmol, 0.05mmol, 0.025mmol, and 0.0125mmol of the compound represented by formula II, respectively, that is, the molar ratio of gold to ligand (Au:ligand) is 1:2, 1:1, 2:1, 4:1, and 8:1, respectively. Different thiol PEG addition amounts are set, so that the molar ratio of thiol PEG to ligand (PEG:ligand) is 0.01:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively, corresponding to 1%, 2%, 5%, 10%, and 20%, respectively; for example: when the ligand solution contains 0.2mmol of the compound represented by formula II, and the thiol PEG solution contains 0.04mmol of thiol PEG, then PEG:ligand is 20%.
[0099] The MIC value test results of gold nanoparticles are as follows Figure 2 shown.
[0100] Effect of the compound represented by formula III (ligand 39) on the antibacterial properties of gold nanoparticles
[0101] Nanogold particles were prepared using the compound represented by formula III (CAS number: 155559-81-2), and the effect of synthesis conditions on the antibacterial properties of nanogold particles was investigated by the orthogonal method.
[0102]
[0103] The preparation of gold nanoparticles was carried out in an ice water bath. The specific steps are as follows:
[0104] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (dissolved in methanol) and 5mL of thiol PEG solution (dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in an ice-water bath for one hour. The reaction solution is dialyzed with deionized water (14kDa MW cut-toff, Millipore) for 72h and sterilized with a 0.22μm filter (Millipore) to obtain nanogold particles.
[0105] Wherein, different ligand addition amounts are set, and the ligand solution contains 0.2mmol, 0.1mmol, 0.05mmol, 0.025mmol, and 0.0125mmol of the compound represented by formula III, respectively, that is, the molar ratio of gold to ligand (Au:ligand) is 1:2, 1:1, 2:1, 4:1, and 8:1, respectively. Different thiol PEG addition amounts are set, so that the molar ratio of thiol PEG to ligand (PEG:ligand) is 0.01:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively, corresponding to 1%, 2%, 5%, 10%, and 20%, respectively; for example: when the ligand solution contains 0.2mmol of the compound represented by formula III, and the thiol PEG solution contains 0.04mmol of thiol PEG, then PEG:ligand is 20%.
[0106] The MIC value test results of gold nanoparticles are as follows Figure 3 shown.
[0107] Effect of the compound represented by formula IV (ligand 27) on the antibacterial properties of gold nanoparticles
[0108] The compound represented by formula IV (CAS number 2268-79-3) was used as a ligand to prepare gold nanoparticles, and the effect of synthesis conditions on the antibacterial properties of gold nanoparticles was investigated by the orthogonal method.
[0109]
[0110] The preparation of gold nanoparticles was carried out in an ice water bath. The specific steps are as follows:
[0111] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (dissolved in methanol) and 5mL of thiol PEG solution (dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in an ice-water bath for one hour. The reaction solution is dialyzed with deionized water (14kDa MW cut-toff, Millipore) for 72h and sterilized with a 0.22μm filter (Millipore) to obtain nanogold particles.
[0112] Wherein, different ligand addition amounts are set, and the ligand solution contains 0.2mmol, 0.1mmol, 0.05mmol, 0.025mmol, and 0.0125mmol of the compound represented by formula IV, respectively, that is, the molar ratio of gold to ligand (Au:ligand) is 1:2, 1:1, 2:1, 4:1, and 8:1, respectively. Different thiol PEG addition amounts are set, so that the molar ratio of thiol PEG to ligand (PEG:ligand) is 0.01:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively, corresponding to 1%, 2%, 5%, 10%, and 20%, respectively; for example: when the ligand solution contains 0.2mmol of the compound represented by formula IV, and the thiol PEG solution contains 0.04mmol of thiol PEG, then PEG:ligand is 20%.
[0113] The MIC value test results of gold nanoparticles are as follows Figure 4 shown.
[0114] Effect of the compound represented by formula V (ligand 38) on the antibacterial properties of gold nanoparticles
[0115] Gold nanoparticles were prepared using the compound represented by formula V as a ligand (CAS No. 80087-71-4), and the effect of synthesis conditions on the antibacterial properties of gold nanoparticles was investigated by an orthogonal method.
[0116]
[0117] The preparation of gold nanoparticles was carried out in an ice water bath. The specific steps are as follows:
[0118] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (dissolved in methanol) and 5mL of thiol PEG solution (dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in an ice-water bath for one hour. The reaction solution is dialyzed with deionized water (14kDa MW cut-toff, Millipore) for 72h and sterilized with a 0.22μm filter (Millipore) to obtain nanogold particles.
[0119] Wherein, different ligand addition amounts are set, and the ligand solution contains 0.2mmol, 0.1mmol, 0.05mmol, 0.025mmol, and 0.0125mmol of the compound represented by formula V, respectively, that is, the molar ratio of gold to ligand (Au:ligand) is 1:2, 1:1, 2:1, 4:1, and 8:1, respectively. Different thiol PEG addition amounts are set, so that the molar ratio of thiol PEG to ligand (PEG:ligand) is 0.01:1, 0.02:1, 0.05:1, 0.1:1, and 0.2:1, respectively, corresponding to 1%, 2%, 5%, 10%, and 20%, respectively; for example: when the ligand solution contains 0.2mmol of the compound represented by formula V, and the thiol PEG solution contains 0.04mmol of thiol PEG, then PEG:ligand is 20%.
[0120] The MIC value test results of gold nanoparticles are as follows Figure 5 shown.
[0121] The appropriate ratio of higher PEG concentration to higher ligand concentration can make the synthesized gold nanoparticles more stable and have better antibacterial properties.
[0122] Example 1
[0123] This example provides a gold nanoparticle (hereinafter referred to as: 6-chloro-2-mercaptobenzothiazole). The preparation is carried out under ice water bath conditions. The specific preparation method is as follows:
[0124] Stir 10 mL of methanol in an ice-water bath for 10 min, add HAuCl4·3H2O solution (41 mg, 0.1 mmol, dissolved in 1 mL of methanol) and stir for 10 min to obtain a light yellow transparent solution. Slowly drop 5 mL of ligand solution (containing 0.2 mmol of the compound shown in formula I, dissolved in methanol) and 5 mL of thiol PEG solution (containing 0.04 mmol of thiol PEG, dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20 min, slowly drop NaBH4 (12 mg, 0.3 mmol, freshly dissolved in 5 mL of methanol), stir vigorously (speed 1500 rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15 min. Then reduce the stirring speed (speed 600 rpm), and continue stirring in the ice-water bath for one hour. The reaction solution was dialyzed with deionized water (14 kDa MW cut-toff, Millipore) for 72 h and sterilized with a 0.22 μm filter (Millipore) to obtain gold nanoparticles.
[0125] Example 2
[0126] This example provides a gold nanoparticle (hereinafter referred to as: 5-chloro-2-mercaptobenzothiazole). The preparation is carried out under ice water bath conditions. The specific preparation method is as follows:
[0127] Stir 10mL of methanol in an ice-water bath for 10min, add HAuCl4·3H2O solution (41mg, 0.1mmol, dissolved in 1mL of methanol) and stir for 10min to obtain a light yellow transparent solution. Slowly drop 5mL of ligand solution (containing 0.2mmol of the compound shown in formula II, dissolved in methanol) and 5mL of thiol PEG solution (containing 0.04mmol of thiol PEG, dissolved in methanol) in sequence, and the solution immediately turns turbid with light yellow flocs. After stirring for 20min, slowly drop NaBH4 (12mg, 0.3mmol, freshly dissolved in 5mL of methanol), stir vigorously (speed 1500rpm), the solution immediately turns black, then turns dark brown, and continues to stir for 15min. Then reduce the stirring speed (speed 600rpm), and continue stirring in the ice-water bath for one hour. The reaction solution was dialyzed with deionized water (14 kDa MW cut-toff, Millipore) for 72 h and sterilized with a 0.22 μm filter (Millipore) to obtain gold nanoparticles.
[0128] Test Example 1
[0129] The nano-gold particles were diluted to 128 μg / mL with ultrapure water. The average particle size and particle size distribution of the nano-gold particles were measured and recorded using a particle size analyzer. The potential value of the nano-gold particles was measured and recorded using a Malvern potentiometer. The UV-Vis absorption curve was measured using an ultraviolet-visible spectrophotometer (UV-Vis) and the absorption peak position and intensity of the nano-gold particles were recorded.
[0130] The results are as follows Figures 6 to 8 shown.
[0131] The average hydrated particle size of the nano-gold particles in Example 1 is 15.63±6.18 nm, and the potential value is -7.58±1.50 mV; the average hydrated particle size of the nano-gold particles in Example 2 is 11.58±1.36 nm, and the potential value is -16.03±3.56 mV.
[0132] Test Example 2
[0133] In this example, the antibacterial properties of gold nanoparticles were tested.
[0134] (1) The MIC value test results of the gold nanoparticles of Examples 1 to 2 for SE, MRSE, EF, MREF, SH, and MRSH are shown in Table 1.
[0135] Table 1
[0136]
[0137] (2) Time-kill curve test: The experimental method is as follows:
[0138] 1) Preparation of bacterial culture solution: Staphylococcus aureus ATCC 29213 and MRSA were inoculated into LB agar plates respectively, and cultured at 37°C overnight; single colonies were picked and inoculated into LB liquid culture medium, and cultured at 37°C overnight; an appropriate amount of bacterial suspension was taken and diluted with LB liquid culture medium to an appropriate bacterial concentration to obtain a diluted bacterial suspension.
[0139] 2) Preparation of drug solution: Dilute the gold nanoparticles to a certain concentration using LB liquid culture medium to obtain a drug solution.
[0140] 3) Draw a time-kill curve: Add equal volumes of diluted bacterial suspension and drug solution to a 96-well plate. Repeat each treatment group 3 times; in the control group, replace the drug solution with an equal volume of LB liquid culture medium, and take samples every 3 hours to measure bacterial growth.
[0141] For Staphylococcus aureus ATCC 29213: The initial bacterial concentration of Staphylococcus aureus ATCC 29213 is 1×10 6CFU / mL, the concentrations of the gold nanoparticles in Examples 1 and 2 were set to 1 and 2 μg / mL, respectively. The initial bacterial concentration of Staphylococcus aureus ATCC 29213 was 1×10 10 CFU / mL, the effective concentrations of the gold nanoparticles in Examples 1 and 2 were set to 8 μg / mL respectively.
[0142] For MRSA: The initial bacterial concentration of MRSA is 5×10 5 CFU / mL, the concentrations of the gold nanoparticles in Example 1 were set to 2 and 4 μg / mL, respectively, and the concentrations of the gold nanoparticles in Example 2 were set to 1 and 2 μg / mL, respectively. The initial bacterial concentration of MRSA was 1×10 9 CFU / mL, the effective concentrations of the gold nanoparticles in Examples 1 and 2 were set to 8 μg / mL respectively.
[0143] The results are as follows Figures 9-10 shown.
[0144] The antibacterial effects of the gold nanoparticles in Examples 1 to 2 are both concentration-dependent and time-dependent.
[0145] (3) Bacterial growth curve test:
[0146] 1) Preparation of bacterial culture medium: Staphylococcus aureus ATCC 29213 and MRSA were inoculated into LB agar plates respectively and cultured at 37°C overnight; single colonies were picked and inoculated into LB liquid culture medium and cultured at 37°C overnight; appropriate amount of bacterial suspension was taken and diluted with LB liquid culture medium to an appropriate bacterial concentration to obtain a diluted bacterial suspension (concentration of 2×10 5 CFU / mL).
[0147] 2) Preparation of drug solution: Dilute the gold nanoparticles and vancomycin to 2 and 4 μg / mL respectively using LB liquid culture medium to obtain a drug solution.
[0148] 3) Draw bacterial growth curve: Add equal volumes of diluted bacterial suspension and drug solution to a 96-well plate. Repeat 3 times for each treatment group. Replace the drug solution with an equal volume of LB liquid culture medium in the control group, and measure the bacterial growth within 36 hours. The absorbance value (OD) at 600nm represents the bacterial growth.
[0149] The results are as follows Figures 11-12 shown.
[0150] The nano-gold particles of Examples 1-2 can effectively inhibit the growth of Staphylococcus aureus and MRSA.
[0151] Test Example 3
[0152] This case tests the effect of gold nanoparticles on the blood parameters of mice to evaluate their biological effects and safety.
[0153] 9 Balb / c mice (purchased from Guangdong Animal Center, 6-8 weeks, 6-18g, 9 females) were randomly divided into a control group (Control), Example 1 group (6-chloro-2-mercaptobenzothiazole) and Example 2 group (5-chloro-2-mercaptobenzothiazole), 3 mice in each group, and were raised and treated according to the laboratory animal management regulations. The control mice were injected with 200 μL of normal saline through the tail vein; the mice in Example 1 group were injected with 50 mg / kg·bw of the nanogold particles of Example 1 (200 μL) through the tail vein; the mice in Example 2 group were injected with 50 mg / kg·bw of the nanogold particles of Example 2 (200 μL) through the tail vein. After 2 days, blood samples of the mice were collected by eye socket bleeding. Use blood cell analyzers and other equipment to perform routine blood tests on blood samples (including white blood cell count (WBC), red blood cell count (RBC), hemoglobin concentration, platelet count (PLT) and other indicators); use biochemical analyzers and other equipment to perform biochemical indicator tests on blood samples (including serum protein (ALB), liver function indicators (aspartate aminotransferase AST, alanine aminotransferase ALT, etc.), renal function indicators (creatinine CR, urea nitrogen Urea, etc.), serum alkaline phosphatase (ALP), blood uric acid (UA), total protein (TP), etc.).
[0154] The results are as follows Figures 13-14 shown.
[0155] The nano-gold particles of Examples 1 and 2 had little effect on various indicators in the blood of mice, which indicates that the nano-gold particles prepared in the examples of the present invention have good biosafety.
[0156] Test Example 4
[0157] This example tests the antibacterial mechanism of gold nanoparticles.
[0158] The nanogold particles of Example 2 were used to treat the concentration of 1×10 8CFU / mL of Staphylococcus aureus ATCC 29213 or MRSA were treated for 6 hours as the treatment group (NP Treatment); Staphylococcus aureus or MRSA without any treatment was used as the control group (Control). The bacteria were fixed in 0.1M carboxylic acid buffer (pH=7.4) with 2.5% glutaraldehyde for 3 hours, washed twice with PBS, fixed with 0.1% austic acid for 30 minutes, washed three times with PBS, and the samples were gradiently dehydrated using ethanol aqueous solutions of different concentrations (v / v) (ethanol concentrations were 30%, 50%, 70%, 90%, 95%, and 100%), with each dehydration lasting 10 minutes. The dehydrated samples were embedded in Epon812 and polymerized at 60°C for 24 hours. The samples were cut into ultra-thin slices with a thickness of 60-70nm, and the slices were placed on On the coated grid. According to the sample type and the structural features to be observed, adjust the TEM parameters such as acceleration voltage, contrast, aperture size, etc. to obtain the best imaging effect. Use the TEM's focusing system to focus the electron beam on the sample to ensure a clear image. Select the area and collect the image.
[0159] The results are as follows Fig.15 shown.
[0160] Gold nanoparticles had no effect on the integrity of bacterial cell membranes, but abnormal cell wall synthesis, suggesting that gold nanoparticles exert their antibacterial effects by inhibiting cell wall synthesis.
[0161] Test Example 5
[0162] In this case, the antibacterial effect of gold nanoparticles in vivo was tested.
[0163] Twenty-eight female Balb / c mice (purchased from Guangdong Animal Center, 6-8 weeks, 16-18g) were taken. On the first day, 200 mg / kg·bw of cyclophosphamide solution (solvent is normal saline) was injected into the mouse peritoneum. On the fourth day, 150 mg / kg·bw of cyclophosphamide solution was injected into the mouse peritoneum. The injection volume was 0.2 mL to establish a neutrophil-deficient thigh infection model mouse. The thigh infection model mice were randomly divided into 7 groups, 4 mice in each group. After disinfecting the dorsal thigh skin of the mouse with 75% alcohol, MRSA was inoculated in the thigh muscle of the mouse. 0.2 mL of bacterial solution (bacterial concentration was 1×10 9 CFU / mL). Two legs of each mouse were counted, so 8 data points were obtained for each group. The treatment method for each group of mice was as follows:
[0164] (1) Baseline group: 2 hours after MRSA inoculation, the bacterial content in the infected area of the thigh of mice in the baseline group was detected.
[0165] (2) Blank control group (saline): 2 hours after MRSA inoculation, 100 μL of saline was administered subcutaneously to the thigh infection model mice for a total of one administration.
[0166] (3) Positive control group (vanco 20 mg / kg): 2 hours after MRSA inoculation, 20 mg / kg vancomycin (100 μL, solvent: normal saline) was administered subcutaneously to the thigh infection model mice for a total of one administration.
[0167] (4) 2.5 mg / kg group: 2 hours after MRSA inoculation, 2.5 mg / kg of the gold nanoparticles of Example 2 (100 μL, the solvent is normal saline) were administered subcutaneously to the thigh infection model mice for a total of one administration.
[0168] (5) 5 mg / kg group: 2 hours after MRSA inoculation, 5 mg / kg of the gold nanoparticles of Example 2 (100 μL, the solvent is normal saline) were administered subcutaneously to the thigh infection model mice for a total of one administration.
[0169] (6) 10 mg / kg group: 2 hours after MRSA inoculation, 10 mg / kg of the gold nanoparticles of Example 2 (100 μL, the solvent is normal saline) was administered subcutaneously to the thigh infection model mice, for a total of one administration.
[0170] (7) 20 mg / kg group: 2 hours after MRSA inoculation, 20 mg / kg of the gold nanoparticles of Example 2 (100 μL, the solvent is normal saline) were administered subcutaneously to the thigh infection model mice for a total of one administration.
[0171] 24 hours after the injection of the drug, the bacterial content of the infected part of the thigh of the mice in the blank control group, the positive control group, the 2.5 mg / kg group, the 5 mg / kg group, the 10 mg / kg group, and the 20 mg / kg group was detected. The method for detecting the bacterial content of the infected part of the thigh of the mice is as follows: the mice are killed, the thigh muscles are separated under sterile conditions, weighed, placed in 1.5 mL of sterile PBS solution for ice bath homogenization, and after a series of 10-fold dilutions, spread on LB solid culture medium, incubated at 35°C for 18 hours, and then the colonies are counted.
[0172] The results are as follows Fig.16 shown.
[0173] The nanogold particles of Example 2 showed good antibacterial effect in the neutrophil-deficient mouse thigh infection model. Compared with the blank control group, the bacterial content in the leg was reduced by 1.39, 1.61, 1.24 and 1.96 orders of magnitude at the dosage of 2.5 mg / kg, 5 mg / kg, 10 mg / kg and 20 mg / kg of nanogold particles, respectively, while it was only reduced by 0.78 orders of magnitude at the dosage of 20 mg / kg of vancomycin. The nanogold particles of Example 2 have better in vivo antibacterial activity than vancomycin.
[0174] In summary, the gold nanoparticles prepared in the present application have good antibacterial effect.
[0175] The embodiments of the present invention are described in detail above in conjunction with the embodiments, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A method for preparing gold nanoparticles, It is characterized in that The following steps are involved: A first mixed solution of a gold salt, a ligand and a stabilizer is prepared, and a first reaction is carried out to obtain a reaction solution; a second mixed solution containing a reducing agent and the reaction solution is prepared, and a second reaction is carried out to obtain nano-gold particles; The ligand has a structure shown in the following general formula: R 1 Selected from Cl, Br, C 1 ~C 4 An alkane group or a hydroxyl group; R 2 Selected from Cl, Br, C 1 ~C 4 an alkane group or a hydroxyl group.
2. The preparation method according to claim 1, It is characterized in that The gold salt comprises at least one of chloroauric acid, tetrachloroauric acid trihydrate and tetrachloroauric acid tetrahydrate; And / or, the stabilizer includes at least one of thiol PEG, Tween80, and PVP.
3. The preparation method according to claim 1, It is characterized in that The ligand includes at least one of the compounds shown in formula I, the compounds shown in formula II, the compounds shown in formula III, the compounds shown in formula IV, and the compounds shown in formula V. Preferably, the molar ratio of the gold salt to the ligand is 1:0.1-2.5; Preferably, the molar ratio of the ligand to the stabilizer is 1:0.005-0.
25.
4. The preparation method according to claim 1, It is characterized in that The reducing agent includes sodium borohydride; Preferably, the molar ratio of the gold salt to the reducing agent is 1:2-4.
5. A gold nanoparticle, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 4.
6. The gold nanoparticles according to claim 5, It is characterized in that The average hydrated particle size of the nano-gold particles is 8nm to 50nm.
7. An antibacterial composition, It is characterized in that Comprising the gold nanoparticles according to claim 5 or 6.
8. The antibacterial composition according to claim 7, It is characterized in that The antibacterial composition further comprises auxiliary materials or carriers.
9. Use of the nano-gold particles according to claim 5 or 6, or the antibacterial composition according to claim 7 or 8 in the preparation of antibacterial products.
10. The use according to claim 9, It is characterized in that The antibacterial product is selected from medicines, preparations, kits, packaging materials, medical supplies or fabrics.
Citation Information
Patent Citations
Method for qualitatively detecting CU<2+> in solution directly by eye
CN101435778A
Preparation method of gold nanometer particles
CN111940755A
Preparation method for functionalized ligand modified gold nanoparticles
CN112570725A
Gold nanocluster as well as preparation method and application thereof
CN117047098A