A kind of inorganic quick-setting reinforcement slurry for mining and preparation method thereof
By using calcium lignoc sulfonate polycarboxylic acid water reducer containing carboxyl and nitrogen and retarder with terminal carboxyl hyperbranched polyester structure, the problem of the retarder on the strength and compatibility of concrete is solved, and reinforcement is improved Compressive strength and retarding properties of the slurry.
Patent Information
- Application Number
- CN202411310489.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The retarder of existing concrete has a great impact on strength performance and is poorly compatible with different types of cement, water reducing agents, and mineral blends, which limits its wide application.
Polycarboxylic acid water reducer obtained by copolymerizing calcium lignosulfonate, acrylic acid, maleic anhydride and polyethylene glycol containing carboxyl and nitrogen, and organic phosphate retarder with end carboxylic hyperbranched polyester structure , enhance the dispersion and retarding properties of the water reducing agent.
The compressive strength and flexural strength of the reinforced slurry are improved, the dispersion ability is enhanced, the retarding performance is improved, and the problem of poor compatibility is overcome.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of reinforcement slurry, and in particular to an inorganic quick-setting reinforcement slurry for mining and a preparation method thereof. Background Art
[0002] It is necessary to provide a new type of grouting material that meets the reinforcement effect, and use additives that take environmental protection and cost into consideration to improve the physical properties of the slurry to meet the current use needs. Lignin sulfonate is an anionic surfactant and can be used as a water reducer for concrete, but when used in excessive amounts, a large number of bubbles will be generated, thereby reducing the strength of the concrete, and in severe cases causing collapse accidents, which limits the widespread application of lignin sulfonate. In order to meet the requirement that concrete is prohibited from being mixed on site, it is necessary to extend the setting time of concrete, so it is necessary to add a suitable retarder to maintain the fluidity of the concrete and extend its plastic time. The retarders currently used have a strong effect on extending the setting time of concrete, but will have a great impact on the strength properties of concrete, and due to the different adsorption properties of gel materials, the retarder has poor compatibility with different types of cement, water reducers, mineral admixtures, etc., thus limiting the use and development of retarders. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides an inorganic quick-setting reinforcement slurry for mining and a preparation method thereof.
[0004] The object of the present invention can be achieved by the following technical scheme: an inorganic quick-setting reinforcement slurry for mining comprises the following raw materials in parts by weight: 50-60 parts of sulphoaluminate cement clinker, 50-60 parts of gypsum-lime mixture, 2.5-3.0 parts of water reducer, 1.5-1.8 parts of thickener, 1.5-1.8 parts of retarder, 1.0-1.5 parts of accelerator, 1.5-2 parts of redispersible latex powder and 90-108 parts of water.
[0005] The mass ratio of gypsum to lime in the gypsum-lime mixture is 7:1.
[0006] The thickener is sodium carboxymethyl cellulose.
[0007] The quick-setting agent is prepared by mixing alumina clinker, sodium carbonate and quicklime in a mass ratio of 1:1:0.5.
[0008] The redispersible latex powder is ethylene-vinyl acetate copolymer rubber powder.
[0009] The water reducing agent is prepared by the following steps:
[0010] Step A1: Add 2-carboxy-5-nitrobenzenesulfonic acid to acetic acid, then add iron powder, stir at room temperature for 12 hours, filter, wash with saturated brine, extract with ethyl acetate, then remove the solvent by vacuum distillation, and dry to obtain intermediate 1, 2-carboxy-5-nitrobenzenesulfonic acid, acetic acid and iron powder in a ratio of 0.018 mol: 24.4 mL: 0.16 mol;
[0011] During the reaction, the nitro group of 2-carboxy-5-nitrobenzenesulfonic acid is reduced to an amino group to generate intermediate 1. The structure of intermediate 1 is shown below:
[0012]
[0013] Step A2: Add intermediate 1 and sodium hydroxide solution to a three-necked flask, stir for 5-10 minutes, then add sodium nitrite, and finally add concentrated hydrochloric acid. After stirring in an ice bath for 2-3 hours, remove the ice bath, continue stirring for 30 minutes, then add calcium lignin sulfonate, stir at room temperature for 4-5 hours, and dry to obtain intermediate 2. The dosage ratio of intermediate 1, sodium hydroxide solution, sodium nitrite, concentrated hydrochloric acid and calcium lignin sulfonate is 0.1 mol: 50 mL: 0.1-0.15 mol: 4-6 mL: 0.1 mol, the molar concentration of the sodium hydroxide solution is 1 mol / L, and the mass fraction of the concentrated hydrochloric acid is 37%;
[0014] During the reaction, the intermediate 1 first reacts with sodium nitrite and concentrated hydrochloric acid to obtain a product which then reacts with calcium lignin sulfonate to generate calcium lignin sulfonate containing nitrogen and carboxyl groups, namely intermediate 2. The structure of intermediate 2 is shown below:
[0015]
[0016] The structure of calcium lignin sulfonate is shown below:
[0017]
[0018] SL = Sulfonated lignin
[0019] Step A3: In a three-necked flask equipped with a condenser, maleic anhydride, intermediate 2 and deionized water were added, and the mixture was refluxed at 80°C for 1.5 hours. Ammonium persulfate and acrylic acid were then added, and the mixture was refluxed at 80°C for 4-5 hours. Then, polyethylene glycol 400 was slowly added dropwise to the three-necked flask, and the mixture was refluxed for 3 hours. The mixture was then immersed in anhydrous ethanol for 24 hours, and distilled under reduced pressure. The water reducing agent was obtained after drying. The dosage ratio of maleic anhydride, intermediate 2, deionized water, ammonium persulfate, acrylic acid and polyethylene glycol 400 was 3g:10g:5mL:0.07g:1.3mL:3.3g.
[0020] During the reaction, acrylic acid, maleic anhydride and polyethylene glycol are grafted with calcium lignin sulfonate to generate a polycarboxylic acid water reducer containing lignin sulfonate. The obtained water reducer can overcome the defects of calcium lignin sulfonate such as excessive air entrainment and insufficient retarding. By introducing carboxyl groups, sulfonic acid groups and nitrogen into calcium lignin sulfonate, the dispersibility of the water reducer in the reinforcement slurry is enhanced.
[0021] The retarder is prepared by the following steps:
[0022] Step B1: Add deionized water, phosphorous acid and concentrated sulfuric acid to a three-necked flask equipped with a stirrer, start stirring, and after 15-20 minutes, slowly drop triethylenetetramine into the three-necked flask. After the dropwise addition is completed, heat to 105°C, slowly drop formaldehyde, and after the dropwise addition is completed, continue to stir and react for 5 hours, cool to room temperature, and adjust the pH to 5.0 with ammonia water to obtain intermediate a; the amount ratio of deionized water, phosphorous acid, concentrated sulfuric acid, triethylenetetramine, formaldehyde and ammonia water is 4.5g:10.25g:2.5g:2.6g:12.2g:10-20mL, the mass fraction of concentrated sulfuric acid is 98%, and the mass fraction of ammonia water is 26%;
[0023] During the reaction, triethylenetetramine, phosphorous acid and formaldehyde undergo a Mannich reaction to generate a hydroxyl-containing organic phosphate substance, namely intermediate a. The structure of intermediate a is shown below:
[0024]
[0025] Step B2: 2-(4-methoxybenzylene)succinic acid and DMAC were added to a three-necked flask, and under nitrogen protection, intermediate a and p-toluenesulfonic acid were added to the three-necked flask, and the mixture was reacted at 140° C. for 6 h, cooled to room temperature, and rotary evaporated to obtain intermediate b. The dosage ratio of 2-(4-methoxybenzylene)succinic acid, DMAC, intermediate a and p-toluenesulfonic acid was 0.025 mol: 50-60 mL: 0.05 mol: 0.2 g;
[0026] During the reaction, under the catalysis of p-toluenesulfonic acid, the two carboxyl groups of 2-(4-methoxybenzyl)succinic acid react with the hydroxyl groups in intermediate a to generate intermediate b.
[0027] Step B3: Add intermediate b and DMAC to a three-necked flask, start stirring, add p-toluenesulfonic acid and toluene to the three-necked flask under nitrogen protection, then add trimellitic anhydride, stir for 30 minutes, react at 140°C for 8 hours, cool to room temperature, and rotary evaporate to obtain a retarder; the amount ratio of intermediate b, DMAC, p-toluenesulfonic acid, toluene and trimellitic anhydride is 0.1 mol: 100 mL: 0.2 g: 20-30 mL: 0.1 mol;
[0028] During the reaction, trimellitic anhydride reacts with intermediate b, and the anhydride ring opens and reacts with the remaining hydroxyl group in intermediate b to generate a retarder with a terminal carboxyl hyperbranched polyester structure. The acryloxy, anisole and phenyl carboxyl structures in the retarder are similar to those of the water reducer, which increases the compatibility of the two. At the same time, the introduction of the organic phosphate retarder structure can reduce the initial dispersibility of the polycarboxylic acid water reducer at low temperatures and improve the dispersion and slump retention performance of the polycarboxylic acid water reducer at room temperature and high temperature.
[0029] Beneficial effects of the present invention: The raw materials of the inorganic quick-setting reinforcement slurry for mining of the present invention include sulphoaluminate cement clinker, gypsum-lime mixture, water reducer, thickener, retarder, accelerator, redispersible latex powder and water. The synthesized water reducer is a polycarboxylic acid water reducer containing lignin sulfonate obtained by copolymerization of calcium lignin sulfonate containing carboxyl and nitrogen, acrylic acid, maleic anhydride and polyethylene glycol. It can not only overcome the defects of excessive air entrainment and insufficient retarding of calcium lignin sulfonate as a water reducer, but also enhance the dispersibility of the water reducer on the reinforcement slurry due to the large steric hindrance effect, greatly improve the water reduction rate and the compressive strength of the reinforcement slurry; the introduction of calcium lignin containing carboxyl, sulfonic acid and nitrogen not only enhances the dispersibility of the water reducer in the reinforcement slurry and reduces the loss of viscosity of the reinforcement slurry, but also improves the compressive and flexural strength of the reinforcement slurry.
[0030] The synthesized retarder has a terminal carboxyl hyperbranched polyester structure. The acryloxy, anisole and phenyl carboxyl structures in its molecules are similar to those of the water reducer, which increases the compatibility of the retarder with the water reducer and overcomes the problem of poor compatibility of concrete admixtures. At the same time, the organic phosphate retarder structure is introduced, which can reduce the initial dispersibility of the polycarboxylic acid water reducer at low temperatures, improve the dispersion and slump retention performance of the polycarboxylic acid water reducer at normal and high temperatures, effectively delay cement hydration, and has excellent retarding performance for reinforced slurry. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1, a water reducing agent, prepared by the following steps:
[0033] Step A1: Add 2-carboxy-5-nitrobenzenesulfonic acid to acetic acid, then add iron powder, stir at room temperature for 10 hours, filter, wash with saturated brine, extract with ethyl acetate, then remove the solvent by vacuum distillation, and dry to obtain intermediate 1, wherein the amount ratio of 2-carboxy-5-nitrobenzenesulfonic acid, acetic acid and iron powder is 0.018 mol: 24.4 mL: 0.16 mol;
[0034] Step A2: Add intermediate 1 and sodium hydroxide solution to a three-necked flask, stir for 5 minutes, then add sodium nitrite, and finally add concentrated hydrochloric acid. After stirring in an ice bath for 2 hours, remove the ice bath, continue stirring for 30 minutes, then add calcium lignin sulfonate, stir at room temperature for 4 hours, and dry to obtain intermediate 2. The amount ratio of intermediate 1, sodium hydroxide solution, sodium nitrite, concentrated hydrochloric acid and calcium lignin sulfonate is 0.1 mol: 50 mL: 0.1 mol: 4 mL: 0.1 mol, the molar concentration of the sodium hydroxide solution is 1 mol / L, and the mass fraction of concentrated hydrochloric acid is 37%;
[0035] Step A3: In a three-necked flask equipped with a condenser, maleic anhydride, intermediate 2 and deionized water were added, and the mixture was refluxed at 80°C for 1.5 hours. Ammonium persulfate and acrylic acid were then added, and the mixture was refluxed at 80°C for 4 hours. Then, polyethylene glycol 400 was slowly added dropwise to the three-necked flask, and the mixture was refluxed for 3 hours. The mixture was then immersed in anhydrous ethanol for 24 hours, and distilled under reduced pressure. The water reducing agent was obtained after drying. The dosage ratio of maleic anhydride, intermediate 2, deionized water, ammonium persulfate, acrylic acid and polyethylene glycol 400 was 3g:10g:5mL:0.07g:1.3mL:3.3g.
[0036] Example 2, a water reducing agent, prepared by the following steps:
[0037] Step A1: Add 2-carboxy-5-nitrobenzenesulfonic acid to acetic acid, then add iron powder, stir at room temperature for 11 hours, filter, wash with saturated brine, extract with ethyl acetate, then remove the solvent by vacuum distillation, and dry to obtain the intermediate 1, 2-carboxy-5-nitrobenzenesulfonic acid, acetic acid and iron powder in a ratio of 0.018 mol: 24.4 mL: 0.16 mol;
[0038] Step A2: Add intermediate 1 and sodium hydroxide solution to a three-necked flask, stir for 8 minutes, then add sodium nitrite, and finally add concentrated hydrochloric acid. After stirring in an ice bath for 2.5 hours, remove the ice bath, continue stirring for 30 minutes, then add calcium lignin sulfonate, stir at room temperature for 4.5 hours, and dry to obtain intermediate 2. The amount ratio of intermediate 1, sodium hydroxide solution, sodium nitrite, concentrated hydrochloric acid and calcium lignin sulfonate is 0.1 mol: 50 mL: 0.12 mol: 5 mL: 0.1 mol, the molar concentration of the sodium hydroxide solution is 1 mol / L, and the mass fraction of concentrated hydrochloric acid is 37%;
[0039] Step A3: In a three-necked flask equipped with a condenser, maleic anhydride, intermediate 2 and deionized water were added, and the mixture was refluxed at 80°C for 1.5 hours. Ammonium persulfate and acrylic acid were then added, and the mixture was refluxed at 80°C for 4.5 hours. Then, polyethylene glycol 400 was slowly added dropwise to the three-necked flask, and the mixture was refluxed for 3 hours. The mixture was then immersed in anhydrous ethanol for 24 hours, and distilled under reduced pressure. The water reducing agent was obtained after drying. The dosage ratio of maleic anhydride, intermediate 2, deionized water, ammonium persulfate, acrylic acid and polyethylene glycol 400 was 3g:10g:5mL:0.07g:1.3mL:3.3g.
[0040] Example 3, a water reducing agent, prepared by the following steps:
[0041] Step A1: Add 2-carboxy-5-nitrobenzenesulfonic acid to acetic acid, then add iron powder, stir at room temperature for 12 hours, filter, wash with saturated brine, extract with ethyl acetate, then remove the solvent by vacuum distillation, and dry to obtain intermediate 1, 2-carboxy-5-nitrobenzenesulfonic acid, acetic acid and iron powder in a ratio of 0.018 mol: 24.4 mL: 0.16 mol;
[0042] Step A2: Add intermediate 1 and sodium hydroxide solution to a three-necked flask, stir for 5-10 minutes, then add sodium nitrite, and finally add concentrated hydrochloric acid. After stirring in an ice bath for 3 hours, remove the ice bath, continue stirring for 30 minutes, then add calcium lignin sulfonate, stir at room temperature for 5 hours, and dry to obtain intermediate 2. The amount ratio of intermediate 1, sodium hydroxide solution, sodium nitrite, concentrated hydrochloric acid and calcium lignin sulfonate is 0.1 mol: 50 mL: 0.15 mol: 6 mL: 0.1 mol, the molar concentration of the sodium hydroxide solution is 1 mol / L, and the mass fraction of concentrated hydrochloric acid is 37%;
[0043] Step A3: In a three-necked flask equipped with a condenser, maleic anhydride, intermediate 2 and deionized water were added, and the mixture was refluxed at 80°C for 1.5 hours. Ammonium persulfate and acrylic acid were then added, and the mixture was refluxed at 80°C for 5 hours. Then, polyethylene glycol 400 was slowly added dropwise to the three-necked flask, and the reaction was refluxed for 3 hours. The mixture was then soaked in anhydrous ethanol for 24 hours, and distilled under reduced pressure. After drying, a water reducer was obtained. The dosage ratio of maleic anhydride, intermediate 2, deionized water, ammonium persulfate, acrylic acid and polyethylene glycol 400 was 3g:10g:5mL:0.07g:1.3mL:3.3g.
[0044] Embodiment 4, a retarder, is prepared by the following steps:
[0045] Step B1: Add deionized water, phosphorous acid and concentrated sulfuric acid to a three-necked flask equipped with a stirrer, start stirring, and after 15 minutes, slowly drop triethylenetetramine into the three-necked flask. After the dropwise addition is completed, heat to 105°C, slowly drop formaldehyde, and after the dropwise addition is completed, continue to stir and react for 5 hours, cool to room temperature, and adjust the pH to 5.0 with ammonia water to obtain intermediate a; the amount ratio of deionized water, phosphorous acid, concentrated sulfuric acid, triethylenetetramine, formaldehyde and ammonia water is 4.5g:10.25g:2.5g:2.6g:12.2g:10mL, the mass fraction of concentrated sulfuric acid is 98%, and the mass fraction of ammonia water is 26%;
[0046] Step B2: 2-(4-methoxybenzylene)succinic acid and DMAC were added to a three-necked flask, and under nitrogen protection, intermediate a and p-toluenesulfonic acid were added to the three-necked flask, and the mixture was reacted at 140° C. for 6 h, cooled to room temperature, and rotary evaporated to obtain intermediate b. The amount ratio of 2-(4-methoxybenzylene)succinic acid, DMAC, intermediate a and p-toluenesulfonic acid was 0.025 mol: 50 mL: 0.05 mol: 0.2 g;
[0047] Step B3: Add intermediate b and DMAC to a three-necked flask, start stirring, add p-toluenesulfonic acid and toluene to the three-necked flask under nitrogen protection, then add trimellitic anhydride, stir for 30 minutes, react at 140°C for 8 hours, cool to room temperature, and rotary evaporate to obtain a retarder; the amount ratio of intermediate b, DMAC, p-toluenesulfonic acid, toluene and trimellitic anhydride is 0.1 mol: 100 mL: 0.2 g: 20 mL: 0.1 mol.
[0048] Example 5, a retarder, prepared by the following steps:
[0049] Step B1: Add deionized water, phosphorous acid and concentrated sulfuric acid to a three-necked flask equipped with a stirrer, start stirring, and after 18 minutes, slowly drop triethylenetetramine into the three-necked flask. After the dropwise addition is completed, heat to 105°C, slowly drop formaldehyde, and after the dropwise addition is completed, continue to stir and react for 5 hours, cool to room temperature, and adjust the pH to 5.0 with ammonia water to obtain intermediate a; the amount ratio of deionized water, phosphorous acid, concentrated sulfuric acid, triethylenetetramine, formaldehyde and ammonia water is 4.5g:10.25g:2.5g:2.6g:12.2g:15mL, the mass fraction of concentrated sulfuric acid is 98%, and the mass fraction of ammonia water is 26%;
[0050] Step B2: 2-(4-methoxybenzylene)succinic acid and DMAC were added to a three-necked flask, and under nitrogen protection, intermediate a and p-toluenesulfonic acid were added to the three-necked flask, and the mixture was reacted at 140° C. for 6 h, cooled to room temperature, and rotary evaporated to obtain intermediate b. The amount ratio of 2-(4-methoxybenzylene)succinic acid, DMAC, intermediate a and p-toluenesulfonic acid was 0.025 mol: 55 mL: 0.05 mol: 0.2 g;
[0051] Step B3: Add intermediate b and DMAC to a three-necked flask, start stirring, add p-toluenesulfonic acid and toluene to the three-necked flask under nitrogen protection, then add trimellitic anhydride, stir for 30 minutes, react at 140°C for 8 hours, cool to room temperature, and rotary evaporate to obtain a retarder; the amount ratio of intermediate b, DMAC, p-toluenesulfonic acid, toluene and trimellitic anhydride is 0.1 mol: 100 mL: 0.2 g: 25 mL: 0.1 mol.
[0052] Example 6, a retarder, prepared by the following steps:
[0053] Step B1: In a three-necked flask equipped with a stirrer, add deionized water, phosphorous acid, and concentrated sulfuric acid, start stirring, and after 20 minutes, slowly drop triethylenetetramine into the three-necked flask, and after the dropwise addition is completed, heat to 105°C, and slowly drop formaldehyde, and after the dropwise addition is completed, continue to stir and react for 5 hours, cool to room temperature, and adjust the pH to 5.0 with ammonia water to obtain intermediate a; the amount ratio of deionized water, phosphorous acid, concentrated sulfuric acid, triethylenetetramine, formaldehyde and ammonia water is 4.5g:10.25g:2.5g:2.6g:12.2g:20mL, the mass fraction of concentrated sulfuric acid is 98%, and the mass fraction of ammonia water is 26%;
[0054] Step B2: 2-(4-methoxybenzylene)succinic acid and DMAC were added to a three-necked flask, and under nitrogen protection, intermediate a and p-toluenesulfonic acid were added to the three-necked flask, and the mixture was reacted at 140° C. for 6 h, cooled to room temperature, and rotary evaporated to obtain intermediate b. The amount ratio of 2-(4-methoxybenzylene)succinic acid, DMAC, intermediate a and p-toluenesulfonic acid was 0.025 mol: 60 mL: 0.05 mol: 0.2 g;
[0055] Step B3: Add intermediate b and DMAC to a three-necked flask, start stirring, add p-toluenesulfonic acid and toluene to the three-necked flask under nitrogen protection, then add trimellitic anhydride, stir for 30 minutes, react at 140°C for 8 hours, cool to room temperature, and rotary evaporate to obtain a retarder; the amount ratio of intermediate b, DMAC, p-toluenesulfonic acid, toluene and trimellitic anhydride is 0.1 mol: 100 mL: 0.2 g: 30 mL: 0.1 mol.
[0056] Example 7, an inorganic quick-setting reinforcement slurry for mining includes the following raw materials by weight: 50 parts of sulphoaluminate cement clinker, 50 parts of gypsum-lime mixture, 2.5 parts of water reducer, 1.5 parts of thickener, 1.5 parts of retarder, 1.0 parts of quick-setting agent, 1.5 parts of redispersible latex powder and 90 parts of water. The mass ratio of gypsum to lime in the gypsum-lime mixture is 7:1. The thickener is sodium carboxymethyl cellulose. The quick-setting agent is a powder prepared by mixing alumina clinker, sodium carbonate and quicklime in a mass ratio of 1:1:0.5. The redispersible latex powder is ethylene-vinyl acetate copolymer powder.
[0057] The inorganic quick-setting reinforcement slurry for mining is prepared by the following steps:
[0058] Add sulphoaluminate cement clinker, gypsum-lime mixture, and the water reducer obtained in Example 1 into a mixer and stir for 15 minutes. Then add a thickener, a retarder obtained in Example 4, an accelerator, and water in sequence and stir for 30 minutes. Then add redispersible latex powder into the mixer and stir for 10 minutes to obtain an inorganic quick-setting reinforcement slurry for mining.
[0059] Example 8, an inorganic quick-setting reinforcement slurry for mining includes the following raw materials by weight: 55 parts of sulphoaluminate cement clinker, 55 parts of gypsum-lime mixture, 2.8 parts of water reducer, 1.6 parts of thickener, 1.6 parts of retarder, 1.2 parts of quick-setting agent, 1.8 parts of redispersible latex powder and 99 parts of water. The mass ratio of gypsum to lime in the gypsum-lime mixture is 7:1. The thickener is sodium carboxymethyl cellulose. The quick-setting agent is a powder prepared by mixing alumina clinker, sodium carbonate and quicklime in a mass ratio of 1:1:0.5. The redispersible latex powder is ethylene-vinyl acetate copolymer powder.
[0060] The inorganic quick-setting reinforcement slurry for mining is prepared by the following steps:
[0061] Add sulphoaluminate cement clinker, gypsum-lime mixture, and the water reducer obtained in Example 2 into a mixer and stir for 18 minutes. Then add a thickener, a retarder obtained in Example 5, an accelerator, and water in sequence and stir for 35 minutes. Then add redispersible latex powder into the mixer and stir for 12 minutes to obtain an inorganic quick-setting reinforcement slurry for mining.
[0062] Example 9, an inorganic quick-setting reinforcement slurry for mining includes the following raw materials by weight: 60 parts of sulphoaluminate cement clinker, 60 parts of gypsum-lime mixture, 3.0 parts of water reducer, 1.8 parts of thickener, 1.8 parts of retarder, 1.5 parts of quick-setting agent, 2 parts of redispersible latex powder and 108 parts of water. The mass ratio of gypsum to lime in the gypsum-lime mixture is 7:1. The thickener is sodium carboxymethyl cellulose. The quick-setting agent is a powder prepared by mixing alumina clinker, sodium carbonate and quicklime in a mass ratio of 1:1:0.5. The redispersible latex powder is ethylene-vinyl acetate copolymer powder.
[0063] The inorganic quick-setting reinforcement slurry for mining is prepared by the following steps:
[0064] Add sulphoaluminate cement clinker, gypsum-lime mixture and the water reducer obtained in Example 3 into a mixer and stir for 20 minutes. Then add thickener, retarder obtained in Example 6, accelerator and water in sequence and stir for 40 minutes. Then add redispersible latex powder into the mixer and stir for 15 minutes to obtain inorganic quick-setting reinforcement slurry for mining.
[0065] Comparative Example 1
[0066] This comparative example is a commercially available inorganic quick-setting reinforcement slurry for mining.
[0067] Comparative Example 2
[0068] Compared with Example 9, the water reducing agent is replaced with calcium lignin sulfonate, and the rest is exactly the same as Example 9 to prepare an inorganic quick-setting reinforcement slurry for mining.
[0069] Comparative Example 3
[0070] Compared with Example 9, the intermediate a used in the preparation process of the retarder obtained in Example 6 is replaced with triethanolamine, and the rest is exactly the same as in Example 9 to obtain an inorganic quick-setting reinforcement slurry for mining.
[0071] The inorganic quick-setting reinforcement slurry for mining prepared by the present invention is further tested for its effect, and the test results are as follows.
[0072] In order to test the inorganic quick-setting reinforcement slurry for mining prepared by the present invention, the performance was measured according to JC / T 2609-2021 "Polymer Cement Reinforced Mortar" and GB / T50080-2002 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", and the results are shown in Table 1.
[0073] Table 1:
[0074]
[0075] According to the data in Table 1, compared with Example 1, Example 7, Example 8 and Example 9, it can be seen that the inorganic quick-setting reinforcement slurry for mining prepared by the present invention has a lower water seepage rate, excellent retarding property, compressive strength and stability compared with the commercially available inorganic quick-setting reinforcement slurry for mining; compared with Example 2, it can be seen that compared with the use of the polycarboxylic acid water reducer introduced with wood sulfonate, the use of only wood sulfonate as a water reducer has insufficient water reduction rate, weakened the compressive strength of the reinforcement slurry, and decreased the stability of the reinforcement slurry; compared with the use of the retarder with a terminal carboxyl hyperbranched polyester structure introduced with an organic phosphate structure, the use of a retarder without an organic phosphate structure to exert a retarding effect, the retarding time is greatly shortened, and the retarding effect is weakened.
[0076] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An inorganic quick-setting reinforcement slurry for mining, characterized in that: The invention comprises the following raw materials in parts by weight: 50-60 parts of sulphoaluminate cement clinker, 50-60 parts of gypsum-lime mixture, 2.5-3.0 parts of water reducer, 1.5-1.8 parts of thickener, 1.5-1.8 parts of retarder, 1.0-1.5 parts of accelerator, 1.5-2 parts of redispersible latex powder and 90-108 parts of water; the mass ratio of gypsum to lime in the gypsum-lime mixture is 7:1, the thickener is sodium carboxymethyl cellulose, the accelerator is alumina clinker, sodium carbonate and quicklime in a mass ratio of 1:1:0.5, and the redispersible latex powder is ethylene-vinyl acetate copolymer rubber powder; The water reducing agent is prepared by the following steps: Step A1: Add 2-carboxy-5-nitrobenzenesulfonic acid to acetic acid, then add iron powder, stir at room temperature for 12 hours, filter, wash with saturated brine, extract with ethyl acetate, and then distill under reduced pressure and dry to obtain intermediate 1; Step A2: Add intermediate 1 and sodium hydroxide solution to a three-necked flask, stir for 5-10 minutes, then add sodium nitrite, and finally add concentrated hydrochloric acid. After stirring in an ice bath for 2-3 hours, remove the ice bath, continue stirring for 30 minutes, then add calcium lignin sulfonate, stir at room temperature for 4-5 hours, and dry to obtain intermediate 2; Step A3: In a three-necked flask equipped with a condenser, add maleic anhydride, intermediate 2 and deionized water, reflux at 80°C for 1.5h, then add ammonium persulfate and acrylic acid, continue to reflux at 80°C for 4-5h, then slowly drop polyethylene glycol 400 into the three-necked flask, continue to reflux for 3h, soak in anhydrous ethanol for 24h, distill under reduced pressure, and dry to obtain a water reducer; The retarder is prepared by the following steps: Step B1: Add deionized water, phosphorous acid and concentrated sulfuric acid to a three-necked flask equipped with a stirrer, start stirring, and after 15-20 minutes, slowly drop triethylenetetramine into the three-necked flask. After the addition is complete, raise the temperature to 105°C, slowly drop formaldehyde, and after the addition is complete, continue stirring and reacting for 5 hours, cool to room temperature, and adjust the pH to 5.0 with ammonia water to obtain intermediate a; Step B2: Add 2-(4-methoxybenzyl)succinic acid and DMAC to a three-necked flask, and under nitrogen protection, add intermediate a and p-toluenesulfonic acid to the three-necked flask, react at 140° C. for 6 h, cool to room temperature, and rotary evaporate to obtain intermediate b; Step B3: Add intermediate b and DMAC to a three-necked flask, start stirring, add p-toluenesulfonic acid and toluene to the three-necked flask under nitrogen protection, then add trimellitic anhydride, stir for 30 minutes, react at 140°C for 8 hours, cool to room temperature, and rotary evaporate to obtain a retarder.
2. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step A1, the usage ratio of 2-carboxy-5-nitrobenzenesulfonic acid, acetic acid and iron powder is 0.018 mol:24.4 mL:0.16 mol.
3. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step A2, the usage ratio of intermediate 1, sodium hydroxide solution, sodium nitrite, concentrated hydrochloric acid and calcium lignin sulfonate is 0.1 mol: 50 mL: 0.1-0.15 mol: 4-6 mL: 0.1 mol, the molar concentration of the sodium hydroxide solution is 1 mol / L, and the mass fraction of the concentrated hydrochloric acid is 37%.
4. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step A3, the usage ratio of maleic anhydride, intermediate 2, deionized water, ammonium persulfate, acrylic acid and polyethylene glycol 400 is 3 g:10 g:5 mL:0.07 g:1.3 mL:3.3 g.
5. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step B1, the dosage ratio of deionized water, phosphorous acid, concentrated sulfuric acid, triethylenetetramine, formaldehyde and ammonia water is 4.5g:10.25g:2.5g:2.6g:12.2g:10-20mL, the mass fraction of concentrated sulfuric acid is 98%, and the mass fraction of ammonia water is 26%.
6. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step B2, the usage ratio of 2-(4-methoxybenzyl)succinic acid, DMAC, intermediate a and p-toluenesulfonic acid is 0.025 mol:50-60 mL:0.05 mol:0.2 g.
7. The inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: In step B3, the usage ratio of intermediate b, DMAC, p-toluenesulfonic acid, toluene and trimellitic anhydride is 0.1 mol:100 mL:0.2 g:20-30 mL:0.1 mol.
8. The method for preparing an inorganic quick-setting reinforcement slurry for mining according to claim 1, characterized in that: Made by the following steps: Add sulphoaluminate cement clinker, gypsum-lime mixture and water reducer into a mixer and stir for 15-20 minutes. Then add thickener, retarder, accelerator and water in sequence and stir for 30-40 minutes. Then add redispersible latex powder into the mixer and stir for 10-15 minutes to obtain inorganic quick-setting reinforcement slurry for mining.