Nylon carbon nanotube graphene aerogel as well as preparation method and application thereof
By preparing nylon/carbon nanotube/graphene aerogels, the problem of uneven dispersion of graphene aerogels in resin composite materials is solved, and the high conductivity and mechanical properties of the composite materials are improved, which is suitable for 3D printing of thermoplastic polyurethane. Material.
Patent Information
- Application Number
- CN202411288014.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Existing graphene aerogels are unevenly dispersed in resin composites, resulting in the composite's electrical conductivity, strength and toughness failing to meet expected requirements.
Using the preparation method of nylon/carbon nanotube/graphene aerogel, first prepare graphene hydrogel to build the gel skeleton structure, then add nylon/carbon nanotube mixed solution, and form a mixed hydrogel through repeated freezing and thawing. Finally, it is freeze-dried and pulverized to improve the compatibility and porosity of the carbon nanotubes and graphene to build a three-dimensional conductive network.
It achieves uniform dispersion of graphene aerogel in thermoplastic polyurethane materials, improves the electrical conductivity and mechanical properties of composite materials, simplifies the production process, and is suitable for the field of 3D printing.
Smart Images

Figure CN118812911A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of honeycomb materials, and in particular relates to a nylon / carbon nanotube / graphene aerogel and a preparation method and application thereof. Background Art
[0002] Functionalization of polymer materials is to give polymer materials new functionality through raw material synthesis or process adjustment. Compared with traditional inorganic materials and metal materials, polymer materials have many advantages such as light weight, high relative strength, good plasticity, low cost, good insulation, etc. Composite materials composed of polymers and functional fillers usually give polymer materials new functionality, and the properties of these polymer composites are determined by the fillers. Fillers can generally be classified into macro fillers, micro fillers and nano fillers according to their size. At the same filler addition amount, nano fillers have a significantly better reinforcing effect on the properties of composite materials than micro fillers and macro fillers, such as electrical conductivity, thermal conductivity and mechanical properties. Under ideal conditions, the higher the mass fraction of nano fillers (for example, graphene, carbon nanotubes or silver nanoparticles) in the polymer, the more obvious the reinforcing effect.
[0003] The traditional way of adding is to blend the functional filler with the polymer matrix. As the content of the functional filler in the polymer matrix increases, it will gradually break through the minimum percolation threshold to form a three-dimensional structure of mutual contact, which is crucial for conductive and thermal conductive polymer composites. After breaking through the minimum percolation threshold, the functional filler forms an effective network structure in the polymer matrix. As the functional filler continues to be added, the rate of increase in the functionality of the composite material begins to rise rapidly. When a certain node is reached, the filler inside the body begins to agglomerate, the rate of increase in the functionality of the composite material begins to decrease, and an uneven distribution of fillers will appear in the polymer matrix, seriously affecting the processing performance and mechanical properties of the polymer composite.
[0004] Graphene is a common conductive reinforcing filler in the field of polymer materials, but the performance of the prepared composite materials has always been unsatisfactory due to problems such as agglomeration of nanomaterials. The three-dimensional graphene macrostructure is made by freeze-drying technology, aiming to develop its low density, high porosity, large specific surface area, super hydrophobicity, excellent mechanical strength and other characteristics. However, there is a problem of uneven dispersion when adding graphene aerogel powder directly. Due to the uneven dispersion of graphene aerogel powder in the resin composite material, the composite material does not meet the expected requirements in terms of conductivity, strength and toughness. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for preparing nylon / carbon nanotube / graphene aerogel, which has excellent compatibility with thermoplastic polyurethane resin and solves the technical problem of uneven dispersion of graphene aerogel powder in resin composite materials.
[0006] The purpose of the present invention can be achieved by the following technical solutions: A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) adding graphene oxide to deionized water to obtain a graphene oxide dispersion, then adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; (2) dissolving nylon powder in a solvent, then adding carbon nanotubes and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder and carbon nanotubes is 1:(0.05-0.3):(1-2); (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, and finally freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel.
[0007] The graphene aerogel continuous network skeleton has good physical properties. When combined with polymer materials such as thermoplastic polyurethane, it can not only enrich the properties of both, but also produce a synergistic effect, giving the composite material excellent performance. Existing graphene aerogel-based polymer composite materials are generally prepared by preforming-impregnation filling method and polymer cross-linking self-assembly method. For example, CN107674421A and CN109810499A respectively prepared composite materials by aerogel preforming and self-assembly process. The above process needs to add a large amount of resin matrix to build a stable gel network, which seriously affects the pore size and porosity of the aerogel itself, resulting in the prepared aerogel being unable to be used as a functional filler.
[0008] In order to solve this problem, the present invention first prepares graphene hydrogel, constructs a gel skeleton structure, and then adds a nylon / carbon nanotube mixed solution to prepare a nylon / carbon nanotube / graphene hydrogel. Carbon nanotubes have high conductivity, light weight, extremely high aspect ratio, and high mechanical strength. The application of carbon nanotubes in polymer-based conductive materials has obvious advantages. When the content in the polymer matrix is relatively low, higher conductivity and mechanical properties can be obtained. The graphene hydrogel prepared in advance plays the role of a matrix, and the carbon nanotubes added subsequently can surround the graphene hydrogel or be immersed in the hydrogel to form a network structure inside or on the surface of the hydrogel, thereby increasing the porosity of the mixed gel and dispersing stress. Further, the two-dimensional graphene is in contact with the one-dimensional carbon nanotube, and a three-dimensional conductive network can be constructed to improve the conductive properties of the composite material.
[0009] In order to improve the compatibility between carbon nanotubes and graphene and polymer matrix, the prior art generally modifies the surface of carbon nanotubes by covalent bonds or non-covalent bonds, reduces the surface energy of carbon nanotubes, and improves the dispersion effect of carbon nanotubes in polymer matrix. Although surface modification can solve the dispersion effect of carbon nanotubes in polymer matrix and improve the electrical and mechanical properties of composite materials, surface modification often involves cumbersome steps, which limits its large-scale application in the industrial field. The present invention adds carbon nanotubes to the mixed solution of nylon, effectively improving the compatibility between carbon nanotubes and graphene; and, when the prepared nylon / carbon nanotube / graphene aerogel is used for 3D printing thermoplastic polyurethane materials, since the amide bond in nylon is similar to the urethane bond structure in polyurethane, it can be used as a connecting bridge to improve the compatibility of graphene / carbon nanotube inorganic materials with polyurethane, eliminating the process steps of modifying graphene / carbon nanotubes. As a resin additive for graphene / carbon nanotube inorganic materials, nylon improves the mechanical properties of aerogel itself on the one hand; on the other hand, it improves the compatibility of aerogel with thermoplastic polyurethane materials, and can promote the dispersion of gel powder in thermoplastic polyurethane during 3D printing. Compared with the polyimide previously used by the inventors, nylon overcomes the technical difficulty of polyimide being difficult to dissolve, and does not require modification using an in-situ polymerization process. It can be directly dissolved and blended with carbon nanotubes, simplifying the production process.
[0010] Moreover, the present invention obtains a mixed hydrogel by repeatedly freezing and thawing the nylon / carbon nanotube / graphene hydrogel dispersion. Furthermore, the number of repeated freezing and thawing is 3-6 times. The freezing device is not particularly limited. The present invention freezes in a refrigerator for 10 hours, then thaws at room temperature for 10 hours, and repeats the freezing / thawing process 4 times to obtain a mixed hydrogel. Through the repeated freezing and thawing process, the fusion of carbon nanotubes and nylon resin with the inner layer of graphene is promoted, and the binding force between the three is enhanced.
[0011] Furthermore, in step (1), the concentration of graphene oxide in the graphene oxide dispersion is 1-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to reducing agent is 1:(0.1-0.5).
[0012] Furthermore, in step (1), the ultrasonic time is 0.5-1h; the reaction temperature is 60-90°C, and the reaction time is 1-4h.
[0013] Furthermore, in step (2), the nylon is at least one of nylon 6, nylon 66, nylon 12, nylon 56, nylon 610, and nylon 1212.
[0014] Furthermore, in step (2), the solvent is at least one of formic acid, sulfuric acid, dimethyl sulfoxide and m-cresol. In order to accelerate the dissolution process, heating and stirring can be performed.
[0015] Furthermore, the carbon nanotubes in step (2) are at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes. The carbon nanotubes are interconnected to form a conductive network. When the amount is too small, an effective conductive network cannot be formed; when the amount is too large, the stability of the gel structure will be destroyed.
[0016] Furthermore, in step (2), the mass ratio of graphene oxide, nylon powder and carbon nanotubes is 1:(0.1-0.3):(1.4-1.7).
[0017] On the other hand, the present invention also provides a nylon / carbon nanotube / graphene aerogel and its application, and uses the nylon / carbon nanotube / graphene aerogel in the field of 3D printing polyurethane materials. The presence of nylon resin improves the compatibility of graphene / carbon nanotube inorganic materials with polyurethane; and the carbon nanotubes distributed on the surface can play the role of "rivets", embedding the gel powder into the polyurethane resin, increasing the bonding force with the polyurethane resin matrix, and improving the conductivity and mechanical properties of the polyurethane composite material.
[0018] The present invention also provides a 3D printing polyurethane material, comprising the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5-10 parts of nylon / carbon nanotube / graphene aerogel; 1-5 parts of flow modifier.
[0019] Thermoplastic polyurethane elastomers have excellent elasticity and strength properties. At room temperature, thermoplastic polyurethane elastomers show high elasticity of rubber, and at high temperatures, they have plastic properties of plastic. The physical cross-linking structure in the high temperature system disintegrates and can be processed secondary, which is very suitable for 3D printing process. Nylon / carbon nanotube / graphene aerogel is used as filler for 3D printing thermoplastic polyurethane elastomer. During the melt processing, the thermoplastic polyurethane elastomer can fully infiltrate the nylon / carbon nanotube / graphene aerogel material. The exposed carbon nanotubes on the surface of the aerogel can play a riveting role, fixing the aerogel to the thermoplastic polyurethane elastomer, and the nylon material in the aerogel further improves its compatibility with the thermoplastic polyurethane elastomer. The addition of nylon / carbon nanotube / graphene aerogel not only enhances the mechanical properties of thermoplastic polyurethane elastomer, but also improves its conductivity. It has a wide range of applications in antistatic materials, microwave absorption and other fields.
[0020] Beneficial effects: The process of the present invention is advanced, simple, energy-saving and time-saving. First, graphene hydrogel is prepared to construct a gel skeleton structure, and then a nylon / carbon nanotube mixed solution is added to prepare a nylon / carbon nanotube / graphene hydrogel. Adding carbon nanotubes to the mixed solution of nylon effectively improves the compatibility between carbon nanotubes and graphene; the amide bond in nylon is similar to the urethane bond structure in polyurethane, which can be used as a connecting bridge to improve the compatibility of graphene / carbon nanotube inorganic materials with polyurethane, eliminating the process step of modifying graphene / carbon nanotubes. As a resin additive for graphene / carbon nanotube inorganic materials, nylon improves the mechanical properties of aerogel itself on the one hand; on the other hand, it improves the compatibility of aerogel with thermoplastic polyurethane materials, and can promote the dispersion of gel powder in thermoplastic polyurethane during 3D printing, which not only enhances the mechanical properties of thermoplastic polyurethane elastomers, but also improves their conductivity. It has a wide range of applications in antistatic materials, microwave absorption and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron microscope image of the nylon / carbon nanotube / graphene aerogel prepared in Example 5; Figure 2 This is a scanning electron microscope image of the nylon / carbon nanotube / graphene aerogel prepared in Comparative Example 1. DETAILED DESCRIPTION
[0022] The present invention is further described by way of the following examples, which do not limit the present invention in any way. Without departing from the technical solution of the present invention, any modification or change made to the present invention that is easily implemented by a person of ordinary skill in the art will fall within the scope of the claims of the present invention.
[0023] Example 1 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.2; the ultrasonic time is 0.5 h; the reaction temperature is 60 ° C, and the time is 4 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.1:1.4; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0024] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0025] Example 2 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.5; the ultrasonic time is 0.8 h; the reaction temperature is 90 ° C, and the time is 1 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.3:1.7; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0026] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 7 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0027] Example 3 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.4; the ultrasonic time is 1 h; the reaction temperature is 80 ° C, and the time is 2 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.3:1.4; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is finally freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 3 times.
[0028] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0029] Example 4 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1.2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.2; the ultrasonic time is 0.6 h; the reaction temperature is 70 ° C, and the time is 3 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.1:1.7; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0030] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 1 part of zinc stearate.
[0031] Example 5 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1.6 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the ultrasonic time is 0.8 h; the reaction temperature is 80 ° C, and the time is 2 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.2:1.6; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0032] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0033] Example 6 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1.6 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the ultrasonic time is 0.8 h; the reaction temperature is 80 ° C, and the time is 2 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.05:1.6; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0034] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0035] Example 7 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1.6 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the ultrasonic time is 0.8 h; the reaction temperature is 80 ° C, and the time is 2 h; (2) Dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.2:1; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0036] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0037] Example 8 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene hydrogel solution; the graphene oxide concentration in the graphene oxide dispersion is 1.6 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:0.3; the ultrasonic time is 0.8 h; the reaction temperature is 80 ° C, and the time is 2 h; (2) dissolving nylon powder in a solvent, then adding multi-walled carbon nanotubes, and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder, and carbon nanotubes is 1:0.2:2; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0038] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0039] Comparative Example 1 A method for preparing nylon / carbon nanotube / graphene aerogel comprises the following steps: (1) Adding graphene oxide and multi-walled carbon nanotubes to deionized water to obtain a graphene oxide / carbon nanotube dispersion, adding a reducing agent to the graphene oxide / carbon nanotube dispersion, ultrasonically treating, and sealing the reaction to obtain a graphene / carbon nanotube hydrogel solution; the graphene oxide concentration in the graphene oxide / carbon nanotube dispersion is 1.6 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to reducing agent is 1:0.3; the ultrasonic time is 0.8 h; the reaction temperature is 80°C, and the time is 2 h; the mass ratio of graphene oxide to carbon nanotubes is 1:1.6; (2) Dissolving nylon powder in a solvent and stirring evenly to obtain a nylon mixed solution; the mass ratio of graphene oxide to nylon powder is 1:0.2; the nylon is nylon 66; and the solvent is formic acid; (3) under stirring conditions, adding the nylon mixed solution dropwise into the graphene / carbon nanotube hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, which is then freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel; the repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
[0040] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0041] Comparative Example 2 The components and preparation process are basically the same as those in Example 5, except that in step (2), the mass ratio of graphene oxide, nylon powder and carbon nanotubes is 1:0.6:1.6.
[0042] A 3D printing polyurethane material comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 6 parts of nylon / carbon nanotube / graphene aerogel; and 2 parts of zinc stearate.
[0043] Performance test: The 3D printed polyurethane materials in Examples 1-8 and Comparative Examples 1-2 were printed into strips, and the tensile properties of the strips were tested with reference to GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber, and the volume resistivity of the 3D printed polyurethane materials was tested using a resistance tester.
[0044] Figure 1 This is a scanning electron microscope image of the nylon / carbon nanotube / graphene aerogel prepared in Example 5. From the image, it can be clearly seen that the graphene sheet structure inside the aerogel is mainly carbon nanotubes outside, the carbon nanotubes are evenly dispersed, and some carbon nanotubes are inserted into the graphene aerogel under the bonding effect of the nylon resin, forming a larger pore size and more uniform porosity. Figure 2 This is a scanning electron microscope image of the nylon / carbon nanotube / graphene aerogel prepared in Comparative Example 1. Figure 2 It shows that directly blending carbon nanotubes and graphene oxide to prepare aerogels will cause graphene and carbon nanotubes to agglomerate, resulting in a decrease in the porosity of the aerogel. The carbon nanotubes cannot form a network structure and cannot effectively disperse the matrix stress, resulting in a decrease in the mechanical properties of the composite material.
[0045] Examples 1-8 show that the present invention first prepares graphene hydrogel, constructs a gel skeleton structure, and then adds a nylon / carbon nanotube mixed solution to prepare a nylon / carbon nanotube / graphene hydrogel. The graphene hydrogel prepared in advance acts as a matrix, and the carbon nanotubes added subsequently can surround the graphene hydrogel or be immersed in the hydrogel to form a network structure inside or on the surface of the hydrogel, thereby increasing the porosity of the mixed gel and dispersing stress. Furthermore, the two-dimensional graphene is in contact with the one-dimensional carbon nanotube, and a three-dimensional conductive network can be constructed to improve the conductive properties of the composite material. It can also be seen from Table 1 that the present invention adds carbon nanotubes to a mixed solution of nylon, which effectively improves the compatibility between carbon nanotubes and graphene; and when the prepared nylon / carbon nanotube / graphene aerogel is used for 3D printing of thermoplastic polyurethane materials, since the amide bond in nylon is similar to the urethane bond structure in polyurethane, it can be used as a connecting bridge to improve the compatibility of graphene / carbon nanotube inorganic materials with polyurethane. The presence of nylon resin improves the compatibility of graphene / carbon nanotube inorganic materials with polyurethane; and the carbon nanotubes distributed on the surface can act as "rivets" to embed the gel powder into the polyurethane resin, increase the bonding force with the polyurethane resin matrix, and improve the conductivity and mechanical properties of the polyurethane composite material. Comparative Example 2 shows that although nylon has a connecting effect, the riveting ability is insufficient when the amount is small; but its amount should not be too much, otherwise it will reduce the porosity of the aerogel, which is not conducive to the infiltration process of the polyurethane material during 3D printing, and reduce the mechanical properties and antistatic properties of the composite material.
[0046] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for preparing nylon / carbon nanotube / graphene aerogel, characterized in that: The following steps are involved: (1) adding graphene oxide to deionized water to obtain a graphene oxide dispersion, adding a reducing agent to the graphene oxide dispersion, ultrasonically treating the dispersion, and sealing the reaction to obtain a graphene hydrogel solution; (2) dissolving nylon powder in a solvent, then adding carbon nanotubes and stirring evenly to obtain a nylon / carbon nanotube mixed solution; the mass ratio of graphene oxide, nylon powder and carbon nanotubes is 1:(0.05-0.3):(1-2); (3) under stirring conditions, adding the nylon / carbon nanotube mixed solution dropwise into the graphene hydrogel solution to prepare a nylon / carbon nanotube / graphene hydrogel dispersion; (4) The nylon / carbon nanotube / graphene hydrogel dispersion is repeatedly frozen and thawed to obtain a mixed hydrogel, and finally freeze-dried and crushed to obtain a nylon / carbon nanotube / graphene aerogel.
2. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: Step (1) The concentration of graphene oxide in the graphene oxide dispersion is 1-2 mg / mL; the reducing agent is ascorbic acid, and the mass ratio of graphene oxide to the reducing agent is 1:(0.1-0.5).
3. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: In step (1), the ultrasonic time is 0.5-1h; the reaction temperature is 60-90°C and the time is 1-4h.
4. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: In step (2), the nylon is at least one of nylon 6, nylon 66, nylon 12, nylon 56, nylon 610, and nylon 1212.
5. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: The solvent in step (2) is at least one of formic acid, sulfuric acid, dimethyl sulfoxide and m-cresol.
6. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: In step (2), the carbon nanotubes are at least one of single-walled carbon nanotubes and multi-walled carbon nanotubes.
7. The method for preparing nylon / carbon nanotube / graphene aerogel according to claim 1, characterized in that: In step (2), the mass ratio of graphene oxide, nylon powder and carbon nanotubes is 1: (0.1-0.3): (1.4-1.7); in step (4), repeated freezing and thawing is performed by freezing in a refrigerator for 10 hours and then thawing at room temperature for 10 hours, and the freezing / thawing process is repeated 4 times.
8. A nylon / carbon nanotube / graphene aerogel, characterized in that: The aerogel is prepared by the method for preparing a nylon / carbon nanotube / graphene aerogel according to any one of claims 1 to 7.
9. A use of the nylon / carbon nanotube / graphene aerogel as claimed in claim 8, characterized in that: Using nylon / carbon nanotube / graphene aerogel in the field of 3D printing polyurethane materials.
10. A 3D printing polyurethane material, characterized in that: The invention comprises the following components in parts by weight: 100 parts of thermoplastic polyurethane elastomer; 5-10 parts of nylon / carbon nanotube / graphene aerogel; and 1-5 parts of flow modifier; the nylon / carbon nanotube / graphene aerogel is the nylon / carbon nanotube / graphene aerogel according to claim 8.
Citation Information
Patent Citations
Method for preparing graphene / carbon nanotube aerogel polymer conductive composite material and application thereof
CN107674421A
Preparation method of graphene aerogel and graphene-carbon nanotube aerogel
CN104401977A
Preparation method of low cost graphene / CNTs aerogel for adsorption of heavy metal ions
CN108905981A
Preparation method of carbon nanotube graphene composite aerogel
CN110155987A
Graphene aerogel based on 3D printing and preparation method thereof
CN112811930A
Cited By
Gel powder with interpenetrating network structure as well as preparation method and application of gel powder
CN119161600A
A gel powder with interpenetrating network structure and its preparation method and application
CN119161600B
A high-performance interpenetrating network structure gel powder and its preparation method and application
CN119192610B
A high-porosity interpenetrating network structure gel powder and its preparation method and application
CN119192665B
Modified interpenetrating network structure gel powder as well as preparation method and application thereof
CN119241904A