Composite steel for ice skate blade and preparation method thereof

Through the composite material and heat treatment technology of high carbon chromium steel and stainless steel, the problem of the advantages and disadvantages of each skate material is solved, the high hardness, corrosion resistance and impact resistance toughness of the skate are achieved, and the service life of the skate is extended.

CN118832918AActive Publication Date: 2024-10-25ZHEJIANG JISEN METAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410761629.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-25
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Existing skate blade materials have their own advantages and disadvantages, and it is difficult to balance high hardness, corrosion resistance and impact resistance, resulting in problems such as frequent sharpening or easy rusting of the skate blades during use.

Method used

It is made of high carbon chromium steel and stainless steel composite materials. The center is high carbon chromium steel and the two sides are stainless steel. Through heat treatment and three-layer composite process, a composite steel for skate blades with a hardness of over HRC60 is formed, which combines wear resistance, oxidation resistance and Impact toughness.

Benefits of technology

It achieves the high hardness, corrosion resistance and impact toughness of the skate material, with an elongation of more than 5%. It has good anti-corrosion performance and oxidation resistance, extending the service life of the skate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118832918A_ABST
    Figure CN118832918A_ABST
Patent Text Reader

Abstract

The invention discloses composite steel for an ice skate blade and a preparation method of the composite steel. The composite steel for the ice skate blade comprises an upper layer and a lower layer, an intermediate layer; a lower layer; wherein the upper layer and the lower layer are made of stainless steel materials; and the middle layer is made of a high-carbon chromium steel material. And the high-carbon chromium steel material of the middle layer comprises the following chemical components: 1.20% of C, 0.3% of Si, 0.5% of Mn, 14.5% of Cr, 4.0% of Mo and 1.2% of V. The stainless steel material of the upper layer 11 and the lower layer 13 comprises the following chemical components: 0.03% of C, 0.3% of Si, 0.5% of Mn, 17.5% of Cr, 12% of Ni and 2.0% of Mo. According to the prepared composite steel for the ice skate blade, a rear blade of the ice skate blade has wear resistance and sharpness retentivity, and the whole ice skate blade can have good toughness, plasticity and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite steel and preparation thereof, and in particular to composite steel for ice skates and a preparation method thereof. Background Art

[0002] With the booming winter tourism industry in cities such as Heilongjiang and Harbin, as well as the hot development of various ice sports competitions, the multi-level ice and snow economic system has been gradually improved, and the development of the ice and snow economy has entered the fast lane. According to the "China Ice and Snow Industry Development Research Report (2023)", the total scale of my country's ice and snow industry is expected to reach 1 trillion yuan in 2025.

[0003] Ice skating is an important part of ice and snow sports. When people mention ice skating, they will think of ice skates and ice blades. With the development of the ice and snow economy, the demand for ice skates and ice blades has increased significantly. As an important part of ice skates, ice skates are usually made of several materials: high carbon steel, alloy chromium steel and stainless steel. Each material has its own characteristics. The hardness of high carbon steel can reach 56-60HRC, and it can remain sharp after long-term use. It is loved by many professional skaters and skating enthusiasts. Its disadvantages are that it is easy to rust and maintenance is more troublesome. Alloy chromium steel: The hardness of alloy chromium steel can reach about 60HRC, and it has certain corrosion resistance. However, chromium steel has poor toughness and is prone to cracks. Stainless steel has good corrosion resistance and is not easy to rust, but its disadvantage is that the hardness is relatively low, which can only reach about 58HRC, and it needs frequent sharpening to keep it sharp. Because different materials have different advantages and disadvantages, ice skate manufacturers have been thinking about how to combine the advantages of various materials to produce ice skates with better performance. In this context, it is necessary to study the steel used for ice skates.

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a composite steel for ice skates and a preparation method thereof:

[0005] 1) The material is a composite of high carbon chromium steel and stainless steel, with the core being high carbon chromium steel. The hardness after heat treatment can reach above HRC60, and it has good oxidation resistance;

[0006] 2) The structural design is as follows: both sides are made of stainless steel, which has good corrosion resistance and impact toughness; after the two materials are compounded, the new material has the excellent properties of both high-carbon chromium steel and stainless steel, and at the same time has better comprehensive performance: wear resistance, oxidation resistance, corrosion resistance and impact toughness. Summary of the invention

[0007] The object of the present invention is to provide a composite steel for ice skates and a preparation method thereof.

[0008] Composite steel for ice skates and preparation method thereof of the present invention:

[0009] The material is a composite of high carbon chromium steel and stainless steel, with the core being high carbon chromium steel. The hardness after heat treatment can reach above HRC60, and it has good oxidation resistance.

[0010] The structural design is as follows: both sides are made of stainless steel, which has good corrosion resistance and impact toughness; after the two materials are compounded, the new material has the excellent properties of both high-carbon chromium steel and stainless steel, and at the same time has better comprehensive properties: wear resistance, oxidation resistance, corrosion resistance and impact toughness.

[0011] A composite steel for ice skates, the composite steel for ice skates comprising:

[0012] upper layer;

[0013] Middle layer;

[0014] Lower level;

[0015] in,

[0016] The upper and lower layers are made of stainless steel;

[0017] The middle layer is made of high carbon chromium steel.

[0018] As a further improvement of the present invention, the thickness of the composite steel used for ice skates is 3.5 to 4.5 mm.

[0019] As a further improvement of the present solution, the intermediate high carbon chromium steel accounts for 40% to 60% of the thickness of the composite material.

[0020] As a further improvement of the present solution, the total thickness of the composite billet of the composite steel for ice skates is a, satisfying the quantitative relationship: a≥25mm.

[0021] As a further improvement of this solution, the chemical composition of the high carbon chromium steel material of the middle layer is: C: 1.20%, Si: 0.3%, Mn: 0.5%, Cr: 14.5%, Mo: 4.0%, V: 1.2%.

[0022] As a further improvement of the present solution, the chemical composition of the stainless steel material of the upper layer 11 and the lower layer 13 is: C: 0.03%, Si: 0.3%, Mn: 0.5%, Cr: 17.5%, Ni: 12%, and Mo: 2.0%.

[0023] A method for preparing composite steel for ice skates, comprising the following preparation steps:

[0024] S1 Pretreatment of raw materials before compounding and compounding

[0025] S11 Pretreatment of raw materials

[0026] Before compounding, use milling and grinding to make the interface to be compounded flat and smooth, and expose the metal color completely, and then use acetone or alcohol to remove foreign matter on the flat surface;

[0027] S12 Composite of raw materials after pretreatment

[0028] The interface between the side and end faces of the composite blank is sealed by welding;

[0029] S2 hot rolling

[0030] The composite blank is hot rolled to form the three-layer composite material into a whole;

[0031] The specific operation steps are: heating the composite blank to 1100-1200°C, keeping the temperature until the temperature inside and outside the composite blank is uniform, and then hot rolling it into a composite strip or plate with a thickness of 3.5-4.5mm;

[0032] S3 recrystallization annealing

[0033] The composite coil after hot rolling in the step is subjected to complete recrystallization annealing at a temperature of 800 to 900° C. The composite coil or plate after annealing is subjected to a pickling or shot blasting process to remove oxide scale to obtain a steel strip with oxide scale removed;

[0034] S4 steel strip trimming

[0035] The steel strip after annealing and removing the surface oxide scale is trimmed, and the welding material welded on the edge when the steel billet is composited is removed to obtain a composite material with a three-layer structure;

[0036] S5 Heat Treatment

[0037] The heat treatment process of composite steel for ice skates includes: quenching + tempering. The quenching temperature is 1080-1130℃, oil cooling.

[0038] As a further improvement of this solution, the quenching temperature in S5 is 1080-1130°C.

[0039] As a further improvement of this solution, the tempering temperature is 150-180°C.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] Compared with the prior art, the composite steel for ice skates of the present invention has the following beneficial effects:

[0042] 1) The composite steel for ice skates of the present invention adopts a three-layer composite process, with high carbon chromium steel in the middle and stainless steel on both sides. The hardness of high carbon chromium steel can reach more than 60HRC after heat treatment, and the PREN value can reach 27; the stainless steel on both sides has high toughness and plasticity, and the elongation of the composite steel reaches more than 5%;

[0043] 2) The manufacturing method of the composite steel for ice skates of the present invention adopts a three-layer composite process, wherein the middle is high-carbon chromium steel and the two side surfaces are stainless steel. The total thickness of the composite billet is controlled to be ≥25 mm, which can ensure that the composite billet has a sufficient reduction ratio to achieve metallurgical bonding when hot-rolled to ≤4.5 mm;

[0044] 3) The manufacturing method of the composite steel for ice skates of the present invention adopts a three-layer composite process, wherein the middle is high-carbon chromium steel and the two side surfaces are stainless steel, wherein the thickness ratio of the high-carbon chromium steel is 40-60%, which can ensure that the thickness of the high-carbon chromium steel in the middle reaches more than 1.4 mm, meeting the thickness requirement of the ice skate blade, and the elongation reaches more than 5%;

[0045] 4) A method for manufacturing composite steel for ice skates, using a three-layer composite process, with high carbon chromium steel in the middle and stainless steel on both sides, with a simple production process and high feasibility. The composite steel ice skates made by this method have wear-resistant blades and sharp retention, and the entire ice skate has good toughness, plasticity and good corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a schematic diagram of the composite steel structure for ice skates of the present invention;

[0047] Description of reference numerals:

[0048] 11-Upper level;

[0049] 12-middle layer;

[0050] 13-Lower level. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described below in conjunction with embodiments:

[0052] The composite steel for ice skates of the present invention adopts a three-layer composite process, and the specific results and preparation method are as follows:

[0053] like Figure 1 As shown, a composite steel for ice skates, the composite steel for ice skates includes:

[0054] upper layer 11; middle layer 12; lower layer 13;

[0055] in,

[0056] The upper layer 11 and the lower layer 13 are both made of stainless steel;

[0057] The middle layer 12 is made of high carbon chromium steel.

[0058] As a preferred embodiment, the thickness of the composite steel for ice skates is 3.5 to 4.5 mm.

[0059] As a preferred embodiment, the intermediate high carbon chromium steel accounts for 40% to 60% of the thickness of the composite material.

[0060] As a preferred embodiment, the total thickness of the composite blank of the composite steel for ice skates is a, satisfying the quantitative relationship: a≥25mm.

[0061] As a preferred embodiment, the chemical composition of the high carbon chromium steel material of the intermediate layer 12 is: C: 1.20%, Si: 0.3%, Mn: 0.5%, Cr: 14.5%, Mo: 4.0%, V: 1.2%.

[0062] As a preferred embodiment, the chemical composition of the stainless steel material of the upper layer 11 and the lower layer 13 is: C: 0.03%, Si: 0.3%, Mn: 0.5%, Cr: 17.5%, Ni: 12%, Mo: 2.0%.

[0063] A method for preparing composite steel for ice skates, comprising the following preparation steps:

[0064] S1 Pretreatment of raw materials before compounding and compounding

[0065] S11 Pretreatment of raw materials

[0066] Before compounding, use milling and grinding to make the interface to be compounded flat and smooth, and expose the metal color completely, and then use acetone or alcohol to remove foreign matter on the flat surface;

[0067] S12 Composite of raw materials after pretreatment

[0068] The interface between the side and end faces of the composite blank is sealed by welding;

[0069] S2 hot rolling

[0070] The composite blank is hot rolled to form the three-layer composite material into a whole;

[0071] The specific operation steps are: heating the composite blank to 1100-1200°C, keeping the temperature until the temperature inside and outside the composite blank is uniform, and then hot rolling it into a composite strip or plate with a thickness of 3.5-4.5mm;

[0072] S3 recrystallization annealing

[0073] The composite coil after hot rolling in the step is subjected to complete recrystallization annealing at a temperature of 800 to 900° C. The composite coil or plate after annealing is subjected to a pickling or shot blasting process to remove oxide scale to obtain a steel strip with oxide scale removed;

[0074] S4 steel strip trimming

[0075] The steel strip after annealing and removing the surface oxide scale is trimmed, and the welding material welded on the edge when the steel billet is composited is removed to obtain a composite material with a three-layer structure;

[0076] S5 Heat Treatment

[0077] The heat treatment process of composite steel for ice skates includes: quenching + tempering. The quenching temperature is 1080-1130℃, oil cooling.

[0078] Among them, the quenching temperature in S5 is 1080~1130℃; the tempering temperature is 150~180℃.

[0079] Structural comments Figure 1 The middle part is high carbon chromium steel, and the surfaces on both sides are stainless steel. The typical chemical composition is shown in Table 1. The high carbon chromium steel in the middle accounts for 40% to 60% of the thickness of the composite material.

[0080] Table 1 Specific material composition in composite steel

[0081]

[0082] The composite steel for ice skates of the present invention provides a composite steel for ice skates having wear resistance, oxidation resistance, corrosion resistance and impact toughness and a method for manufacturing the composite steel.

[0083] After heat treatment, the composite steel for ice skates described in the present invention has a hardness of more than 60HRC at the center, an overall elongation of more than 5%, a pitting resistance index PREN value = Cr+3.3Mo of more than 22, and has good corrosion resistance and oxidation resistance.

[0084] The embodiments and comparative examples are as follows:

[0085] Example:

[0086] The high carbon chromium steel in Table 1 was selected as the central material of the composite blank and used as comparative example 1, and the thickness of comparative example 1 was 4.5 mm; the stainless steel in Table 1 was selected as the two side materials, symmetrically distributed on both sides of the central high carbon chromium steel, and the stainless steel was used as comparative example 2, and the thickness of comparative example 2 was 4.5 mm. High carbon chromium steel and stainless steel of different thicknesses were selected to form composite blanks to form Examples 1 to 6, as shown in Table 2.

[0087] The thickness of the high carbon chromium steel in the center of the blanks of Examples 1 to 6 is 10-40 mm, the thickness of the stainless steel on both sides is 7.5-15 mm, the total thickness of the blanks is 25-70 mm, and the thickness ratio in the center is between 40-60%.

[0088] Before compounding, the interface to be compounded is processed to be flat and smooth by milling and grinding, and the metallic color is completely exposed. Then, foreign matter on the flat surface is removed with acetone or alcohol. The interface of the side and end faces of the composite blank is sealed by welding to avoid oxidation of the composite surface during heating.

[0089] The blanks compounded according to the thickness ratios of 1 to 6 are heated to 1100 to 1200°C, kept warm until the temperature inside and outside the composite blank is uniform, and then hot-rolled into a composite plate with a thickness of 4.5 mm. After ultrasonic inspection, no pores or interlayer defects were detected inside the hot-rolled plate. The interface of the three-layer composite material after hot rolling completely became a whole, achieving metallurgical bonding. It can be seen that when the thickness of the blank reaches more than 25 mm, the hot-rolled thickness ≤ 4.5 mm can ensure that the composite interface achieves a firm metallurgical bonding.

[0090] After hot rolling, the composite coil is subjected to complete recrystallization annealing at a temperature of 870°C, which is then slowly cooled to room temperature after being kept for 8 hours. The hot-rolled plate after annealing is subjected to shot blasting to remove the oxide scale. The steel strip with the surface oxide scale removed is trimmed, and the welding material welded on the edge during the composite billet is removed and set aside.

[0091] The thickness of the center layer of the material after hot rolling in Examples 1 to 6, taking Examples 1 and 4 as examples, is 1.6 mm. It can be seen that the ratio of the center thickness to the total thickness after hot rolling is basically the same as that before hot rolling. The thickness of the ice skate is generally 3.5 to 4.0 mm, and the thickness of the blade of the working part is 1.4 mm. When the thickness of the composite steel material is 3.5 to 4.5 mm and the thickness ratio of the high carbon chromium steel is 40-60%, the thickness of the high carbon chromium steel in the middle can be guaranteed to reach 1.4 mm, which just meets the thickness requirement of the ice skate blade.

[0092] The heat treatment process of composite steel for ice skates includes: quenching + tempering.

[0093] The annealed steel sheets of Examples 1 to 6 were subjected to quenching and tempering heat treatments, with the quenching temperature being 1100° C. and oil cooling to room temperature; the tempering temperature being 160° C. and the tempering time being 4 hours.

[0094] The performance of the samples of Examples 1-6 is shown in Table 3. After quenching at 1100°C and tempering at 160°C, the hardness of the central high carbon chromium steel is 61-62HRC, which is consistent with the hardness of the conventional high carbon chromium steel comparative example 1, and higher than the hardness requirement of the blade of an ordinary ice skate of ≥56HRC. The overall elongation of the samples of Examples 1-6 after heat treatment was tested, and the result showed that the elongation was 5.3-8.1%, which is much higher than the elongation of the conventional high carbon chromium steel comparative example 1. It can be foreseen that the composite steel has good toughness and plasticity.

[0095] Table 2 Processing parameters of Comparative Examples 1-2 and Examples 1-6

[0096]

[0097]

[0098] Table 3 Performance test results of samples of Comparative Examples 1-2 and Examples 1-6

[0099]

[0100] It can be seen from Tables 1 and 2 that the center thickness ratio of Example 1 and Example 4 is 40%, and the elongation of the composite steel is 7.6% and 8.1%; the center thickness ratio of Example 2 and Example 5 is 50%, and the elongation of the composite steel is 6.4% and 6.6%; the center thickness ratio of Example 3 and Example 6 is 57%, and the elongation of the composite steel is 5.4% and 5.8%. As the center thickness ratio increases, the elongation of the composite steel decreases. When the center thickness is not higher than 60%, the elongation of the composite steel can reach more than 5%.

[0101] In the field of stainless steel, the pitting resistance index PREN value = Cr + 3.3Mo represents the corrosion resistance of stainless steel. The higher the value, the stronger the corrosion resistance. When the PREN value reaches 13 or above, it can resist corrosion in the atmospheric environment; when the PREN value reaches 17, it can resist corrosion in a weakly corrosive environment; when the PREN value reaches 21, it can resist corrosion at a certain temperature. The PREN value of the composite steel is calculated according to the chemical composition of the two composite steel raw materials in Table 1, see Table 3. It can be seen that the PREN value of the central material of the composite steel is 27, and the PREN value of the materials on both sides is 23. It can be seen that when the composite steel is made into an ice skate, the central material is used as the blade, and its PREN value is 27, which will have the ability to resist high temperature corrosion and oxidation, while the PREN value of the material on both sides of the ice skate is 23, which also has relatively high corrosion resistance.

[0102] The above experimental analysis shows that after heat treatment, the composite steel for ice skates proposed in this application has a hardness of more than 60HRC at the center, an overall elongation of more than 5%, and a pitting resistance index PREN value = Cr+3.3Mo of more than 22. After being made into ice skates, the blade has wear resistance and sharpness retention, and the whole ice skate has good toughness, plasticity and good corrosion resistance.

[0103] The above embodiments show that the invention steel can achieve more excellent fatigue performance after adopting the above heat treatment process, and is particularly suitable for manufacturing valve plates, and can also be used in other fields with high quality requirements.

[0104] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent changes made using the present invention are within the patent protection scope of the present invention.

Claims

1. A composite steel for ice skates, characterized in that: The composite steel for ice skates includes: Upper layer (11); Middle layer (12); Lower layer (13); in, The upper layer (11) and the lower layer (13) are both made of stainless steel; The middle layer (12) is made of high carbon chromium steel material.

2. The composite steel for ice skates according to claim 1, characterized in that: The thickness of composite steel for ice skates is 3.5 to 4.5 mm.

3. The composite steel for ice skates according to claim 1, characterized in that: The intermediate high carbon chromium steel accounts for 40% to 60% of the thickness of the composite material.

4. The composite steel for ice skates according to claim 1, characterized in that: The total thickness of the composite billet of composite steel for ice skates is a, satisfying the quantitative relationship: a≥25mm.

5. The composite steel for ice skates according to claim 1, characterized in that: The chemical composition of the high carbon chromium steel material of the middle layer (12) is: C: 1.20%, Si: 0.3%, Mn: 0.5%, Cr: 14.5%, Mo: 4.0%, V: 1.2%.

6. The composite steel for ice skates according to claim 1, characterized in that: The chemical composition of the stainless steel material of the upper layer 11 and the lower layer 13 is: C: 0.03%, Si: 0.3%, Mn: 0.5%, Cr: 17.5%, Ni: 12%, Mo: 2.0%.

7. A method for preparing the composite steel for ice skates according to any one of claims 1 to 6, characterized in that: The method comprises the following preparation steps: S1 Pretreatment of raw materials before compounding and compounding S11 Pretreatment of raw materials Before compounding, use milling and grinding to make the interface to be compounded flat and smooth, and expose the metal color completely, and then use acetone or alcohol to remove foreign matter on the flat surface; S12 Composite of raw materials after pretreatment The interface between the side and end faces of the composite blank is sealed by welding; S2 hot rolling The composite blank is hot rolled to form the three-layer composite material into a whole; The specific operation steps are: heating the composite blank to 1100-1200°C, keeping the temperature until the temperature inside and outside the composite blank is uniform, and then hot rolling it into a composite strip or plate with a thickness of 3.5-4.5mm; S3 recrystallization annealing The composite coil after hot rolling in the step is subjected to complete recrystallization annealing at a temperature of 800 to 900° C. The composite coil or plate after annealing is subjected to a pickling or shot blasting process to remove oxide scale to obtain a steel strip with oxide scale removed; S4 steel strip trimming The steel strip after annealing and removing the surface oxide scale is trimmed, and the welding material welded on the edge when the steel billet is composited is removed to obtain a composite material with a three-layer structure; S5 Heat Treatment The heat treatment process of composite steel for ice skates includes: quenching + tempering. The quenching temperature is 1080-1130℃, oil cooling.

8. The method for preparing composite steel for ice skates according to claim 7, characterized in that: The quenching temperature in S5 is 1080-1130°C.

9. The method for preparing composite steel for ice skates according to any one of claims 6 or 7, characterized in that: The tempering temperature is 150-180°C.

Citation Information

Patent Citations

  • Cavitation corrosion resistant dual-phase stainless steel

    CN102011067A

  • Production method of carbon steel workpiece for speed skating ice skate blade

    CN103789630A

  • Multi-layer composite stainless steel material and preparation method thereof

    CN106676410A

  • Steel for low-magnetic high-strength corrosion-resistant fastener and fastener

    CN113737091A

  • Special composite steel with high-hardness steel core for kitchen knife and preparation method of special composite steel

    CN115418574A