Method for producing bearing steel through electric furnace-slagging-off-LF-RH-CC technology
Through the electric furnace-slagging-LF-RH-CC process, the problems of high risk of inclusions and poor purity of molten steel in the electric furnace smelting of bearing steel are solved, and the production of high-carbon steel tapping, low oxygen content and high purity is achieved. Controlling process parameters and using high-alkalinity covering agents reduce aluminum loss and secondary pollution, and improve the purity of the continuous casting process.
Patent Information
- Application Number
- CN202410899245.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-25
AI Technical Summary
The existing electric furnace smelting bearing steel process has problems such as high risk of inclusions and poor purity of molten steel. Especially in the production of high-purity bearing steel, the initial oxygen content increases, aluminum consumption is large, and many inclusions are generated, resulting in a decrease in the purity of molten steel. .
The electric furnace-slagging-LF-RH-CC process is used to control the oxygen content of molten steel and the generation and floating of inclusions through the processes of EAF electric furnace smelting, electric furnace slagging, LF refining, RH refining and CC bloom casting. Use High alkalinity covering agent and carbonized rice husk are used for soft blowing to extend the vacuum time and adjust the circulation flow to improve the purity of molten steel.
It effectively reduces the initial oxygen content, increases the dephosphorization rate and tapping temperature, reduces the generation of inclusions and aluminum loss, improves the purity of molten steel, avoids secondary pollution, and improves the purity of the continuous casting process.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a method for producing bearing steel by adopting an electric furnace-slag removal-LF-RH-CC process. Background Art
[0002] At present, the process flow of electric furnace smelting bearing steel includes electric furnace full scrap steel smelting, deoxidation, alloying, slag making after steel tapping, LF furnace power supply, deoxidation, fine-tuning of alloy, VD or RH vacuum degassing and continuous casting.
[0003] For high-purity bearing steel, when the tapping carbon is lower than 0.15%, the initial oxygen content of the molten steel increases exponentially, the aluminum consumption increases significantly, and the inclusions generated by precipitation deoxidation increase, resulting in a decrease in the purity of the molten steel. The slag from the tapping strip and the filling material at the tapping port entering the ladle will deteriorate the composition of the refined slag. The negative effect of the reduction in the basicity of the refined slag is that the slag's ability to adsorb inclusions is reduced, the aluminum consumption during the smelting process increases, the number of inclusions generated increases, the risk of inclusions increases, and the visibility of the continuous casting molten steel is reduced. RH vacuuming at a large circulation flow for a long time will cause large vacuum aluminum losses, and the purity of the molten steel will decrease after vacuuming.
[0004] The invention patent application with publication number CN116855679A, "A slag-making method for controlling the size of inclusions in the LF refining process of GCr15 bearing steel", adopts VD furnace vacuuming. The characteristics of VD furnace are mixed extraction of steel slag, and the vacuum process is always slag rolling, and the probability of large-sized inclusions is extremely high. In addition, the VD furnace pre-extraction, vacuum process release and mixed extraction of steel slag cause high aluminum loss in the vacuum process, so it is difficult to control the purity of molten steel by vacuuming the VD furnace. In addition to degassing, the VD process is a process that pollutes molten steel. The slag rolling and a large amount of aluminum loss in the VD vacuum process cause a large number of large-particle inclusions to be generated, which are difficult to fully float after vacuuming.
[0005] Therefore, the common process of existing electric furnace smelting bearing steel has high risk of inclusions and poor purity of molten steel, which needs to be solved urgently. Summary of the invention
[0006] In order to solve the problems of high inclusion risk and poor purity of molten steel in the common process of smelting bearing steel in electric furnace, the present invention provides a method for producing bearing steel by adopting electric furnace-slag removal-LF-RH-CC process.
[0007] The technical solution of the present invention:
[0008] A method for producing bearing steel by using an electric furnace-slag removal-LF-RH-CC process, wherein the specific process flow includes EAF electric furnace smelting → electric furnace post-slag removal → LF refining → RH refining → CC large square billet continuous casting, wherein:
[0009] During EAF electric furnace smelting:
[0010] The proportion of 85-95wt% molten iron and 5-15wt% scrap steel is adopted, and the smelting is carried out by full oxygen blowing. After all the scrap steel is melted, lime is added in batches for slagging and dephosphorization, and automatic slag retention is started; when a molten pool is formed in the furnace, carbon oxygen guns at the furnace door are used to spray carbon to form foam slag; after the furnace is fully melted, the temperature is measured and samples are taken, lime is added according to the C and P components, oxygen is blown, and sampling is performed. When the carbon content is 0.30-0.70wt%, P≤0.015wt%, and the temperature is 1610-1640°C, steel is tapped;
[0011] Deoxidation and alloying of steel are carried out and the argon flow rate of the ladle bottom is controlled. After steel is discharged, the argon flow rate of the ladle bottom remains unchanged until the ladle receiving position, and the argon flow rate of the ladle bottom is reduced until the slag removal process begins;
[0012] During the slagging process after the electric furnace:
[0013] The ladle enters the slag removal position, the argon flow rate is adjusted to the argon diameter of the slag surface 300±10mm, the ladle is tilted to the specified position to start slag removal, and the slag removal is completed when the residual slag on the molten steel surface is less than 100mm in diameter, the argon is turned off, and the ladle is transferred to the LF refining ladle receiving position;
[0014] During LF refining:
[0015] The ladle enters the LF refining position, argon is connected, synthetic slag and lime are added, and the slag is melted. 80-100kg / 100 tons of steel SiC is added for diffusion deoxidation during the first power supply. The power supply is 25-30 minutes. The temperature of the molten steel is 1520-1530℃. The refined slag forms white slag. The first full component analysis sample is taken. After the analysis sample is reported, the alloy is fine-tuned according to the composition. The alloy composition and molten steel temperature are adjusted to the process requirements. After the first power supply, 30-50kg / 100 tons of steel SiC is added for diffusion deoxidation. The white slag is maintained. After the temperature and composition meet the requirements of leaving the station, the station leaves and enters the RH;
[0016] During RH refining:
[0017] The ladle enters the RH position, the argon is turned on, the ladle is lifted and vacuum is started, the circulation flow rate is set to 1800NL / min, and the vacuum degree is maintained for 20-30 minutes after ≤67Pa, and then the circulation flow rate is switched to 1200NL / min and maintained for 10 minutes before breaking the air. After breaking the air, carbonized rice husk is added to start soft blowing. The argon flow rate of the first air brick is 20-40NL / min, and the argon flow rate of the second air brick is 60-80NL / min. After 10 minutes of soft blowing, the argon flow rate of the first air brick is adjusted to 60-80NL / min, and the argon flow rate of the second air brick is adjusted to 20-40NL / min. After 5-10 minutes of soft blowing, continuous casting is carried out on the ladle;
[0018] CC bloom continuous casting process:
[0019] After the tundish car is aligned, open the water outlet of the large ladle to inject molten steel into the tundish. When the water outlet of the large ladle is opened, the ladle drainage sand is taken out. When the molten steel in the tundish reaches 1 / 3 of the tundish volume, close the argon flushing of the tundish, and start adding 200-300kg / 100 tons of steel of high alkalinity tundish covering agent into the tundish. After the molten steel in the tundish reaches the working liquid level, add 25-35kg / 100 tons of steel of carbonized rice husk.
[0020] Furthermore, in the EAF electric furnace smelting process, slag dephosphorization is carried out by adding 0.8 to 1.0 ton of lime per 100 tons of steel at the end of the melting period. After full melting, no lime is added according to the slag volume in the furnace and the process requirements for phosphorus in steelmaking. The amount of lime added each time shall not exceed 500 kg per 100 tons of steel.
[0021] Furthermore, during the EAF electric furnace smelting process, the order of steel tapping deoxidation and alloying is to add 0.8 kg / ton of aluminum ingots when 1 / 5 of the steel is tapped, add alloy and increase carbon at the same time when 1 / 3 of the steel is tapped, and add lime and fluorite when 1 / 2 of the steel is tapped.
[0022] Furthermore, during the EAF electric furnace smelting process, the argon gas flow rate of the ladle bottom blowing during the steel tapping process is 700NL / min, and the argon gas flow rate of the ladle bottom blowing at the receiving position is 300-400NL / min.
[0023] Furthermore, during the slag removal process at the rear of the electric furnace, the slag in the middle of the slag surface of the ladle is mainly removed. As the slag in the middle is removed, the surrounding slag is gradually blown to the middle of the ladle by argon gas, and then the slag in the middle continues to be removed, and the operation is repeated.
[0024] Furthermore, during the LF refining process, the argon flow rate is controlled at 300-500 NL / min during the first power supply, and the argon flow rate is controlled at 100-250 NL / min after the first power supply.
[0025] Furthermore, during the LF refining process, the final white slag composition is CaO: 55±2wt%, SiO2≤7wt%, Al2O3: 28~30wt%, MgO≤5wt%, FeO≤0.5wt%, and slag basicity R: 7~9.
[0026] Furthermore, during the RH refining process, 6 to 12 kg / 100 tons of steel of carbonized rice husk is added to the argon position on the slag surface after breaking the air, and argon is blown from the bottom of the ladle for soft blowing.
[0027] Furthermore, during the continuous casting of CC billets, the main components of the high-basicity middle coating agent are CaO: 45-55wt%, SiO2≥5wt%, and Al2O3: 30-35wt%.
[0028] Furthermore, the chemical composition of the bearing steel includes, by weight percentage: C: 0.95-1.05%, Si: 0.15-0.35%, Mn: 0.25-0.45%, Cr: 1.40-1.65%, and the rest is Fe and unavoidable impurities.
[0029] Beneficial effects of the present invention:
[0030] The present invention provides a method for producing bearing steel by adopting an electric furnace-slag stripping-LF-RH-CC process, wherein the electric furnace has a high iron-water ratio smelting, high-carbon steelmaking, and reduced oxygen content in the initial molten steel. The slag flow method is adopted to increase the dephosphorization rate and the steelmaking temperature. Slag stripping after steelmaking can remove the slag in the steelmaking belt and most of the inclusions generated in the steelmaking process, thereby avoiding the secondary pollution of the molten steel by the oxidized slag in the steelmaking belt and improving the purity of the molten steel. The LF furnace quickly forms white slag, and the slag composition is stable. The slag has high basicity and is more efficient in adsorbing inclusions. The RH furnace prolongs the vacuum holding time, reduces the circulation flow, and operates with variable circulation to reduce vacuum aluminum loss. The variable argon flow rate in the soft blowing process can improve the floating efficiency of inclusions and improve the purity of the molten steel after vacuum. The continuous casting whole process is protected and poured, and a high-basicity covering agent is used to effectively avoid secondary oxidation and the contamination of the molten steel in the tundish by the covering agent. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0032] Example 1
[0033] This embodiment provides a method for producing bearing steel by adopting an electric furnace-slag removal-LF-RH-CC process.
[0034] The chemical composition of the bearing steel in this embodiment includes, by weight percentage: C: 0.95-1.05%, Si: 0.15-0.35%, Mn: 0.25-0.45%, Cr: 1.40-1.65%, Al: 0.012-0.020wt%, and the rest is Fe and unavoidable impurities.
[0035] The specific process flow of this embodiment is EAF electric furnace smelting → electric furnace slag removal → LF refining → RH refining → CC large square billet continuous casting, wherein:
[0036] During EAF electric furnace smelting:
[0037] The electric furnace adopts a ratio of 85wt% molten iron and 15wt% scrap steel, and adopts the operation of retaining steel and slag. After adding the materials, it adopts the full oxygen blowing smelting method for blowing. After all the scrap steel is melted, lime is added in batches for slag making and dephosphorization.
[0038] In the dephosphorization operation, 0.8 tons of lime / 100 tons of steel are added at the end of the melting period, and automatic slag flow begins. After full melting, according to the amount of slag in the furnace and the requirements of the process for phosphorus in steel, appropriate amount of lime is added, and the amount added each time shall not exceed 500kg / 100 tons of steel.
[0039] When a molten pool is formed in the furnace, carbon is sprayed from the furnace door carbon-oxygen gun to form foamed slag. The amount of carbon powder sprayed is controlled at 5-50 kg / min according to the foamed slag situation.
[0040] When the furnace is fully melted, the temperature is measured. If the temperature is ≥1580℃, a sample is taken for full analysis. At this time, the C content in the steel is 1.0-2.0wt%, and the P content is 0.020-0.035wt%. After the composition is reported, lime is added and oxygen is blown according to the C and P components. The sample is analyzed. At this time, the C content is 0.40-0.70wt%, and the P content is ≤0.015wt%. The temperature is 1610-1620℃. The steel can be tapped if the composition and temperature are qualified.
[0041] The order of deoxidation and alloying of steel is: add 0.8kg / ton of aluminum ingot to 1 / 5 of the steel, add alloy to 1 / 3 of the steel and increase carbon at the same time, and add lime and fluorite to 1 / 2 of the steel.
[0042] During the steel-discharging process, the argon flow rate of the ladle bottom is controlled at 700NL / min. After the steel is discharged, the argon flow rate of the ladle bottom remains unchanged until the ladle receiving position, and the argon flow rate of the ladle bottom is reduced to 300NL / min, and the argon flow rate remains unchanged until the ladle enters the slag removal process.
[0043] In this embodiment, the number of furnace wall oxygen guns is changed from 3 to 5, all of which are changed to cluster jet oxygen guns, and the oxygen supply intensity of a single gun is increased to a maximum of 2000m 3 / h, which improves oxygen utilization. The full oxygen blowing smelting cycle of the electric furnace is 50-65 minutes / furnace, which is 20-30 minutes shorter than the power supply + oxygen blowing smelting cycle. The carbon content of the steel is increased from the original 0.15% to 0.30-0.70%.
[0044] This embodiment adopts slag flow operation, the dephosphorization rate is increased by more than 30%, and the steel tapping temperature is increased by about 30°C.
[0045] Compared with the full scrap steel mode in which about 30% of pig iron or molten iron is added to smelt bearing steel, the final oxygen content is 180-440ppm, and the amount of aluminum added in the steel is 1.0-1.5kg / ton of steel, the electric furnace operation mode adopted in this embodiment has a final oxygen content of 100-150ppm in the furnace and an aluminum addition of 0.8kg / ton of steel. When the Al composition range of the finished steel is 0.012-0.020wt%, the aluminum consumption is reduced by 0.2-0.7kg / ton of steel and the amount of Al2O3 inclusions produced is reduced by 0.378-1.323kg / ton of steel.
[0046] During the slagging process after the electric furnace:
[0047] The ladle enters the slag removal position, the argon flow rate is adjusted to about 300mm argon diameter on the slag surface, the ladle is tilted to the specified position, and slag removal begins. The slag in the middle of the slag surface of the ladle is mainly removed. As the slag in the middle is removed, the surrounding slag is gradually blown to the middle of the ladle by the argon gas, and then the slag in the middle is continued to be removed. This reciprocating operation is repeated until the residual slag on the steel liquid surface is less than 100mm in diameter, and the slag removal rate is >97%. The argon gas is turned off and the ladle is transferred to the LF refining receiving position.
[0048] The purpose of not shutting off the bottom blowing argon after steel tapping until the end of slag removal is that the entire process from steel tapping and slag addition to the end of slag removal is a process in which inclusions float up. If the argon is shut off, the adsorption efficiency of the slag on inclusions will be reduced.
[0049] During LF refining:
[0050] The ladle enters the LF refining position, argon is connected, synthetic slag and lime are added, and power is supplied for about 3 minutes. After the slag is melted, high-purity SiC is added for diffusion deoxidation.
[0051] The argon flow rate of the first power supply of LF refining is controlled at 300NL / min, and the amount of diffused deoxidized SiC is 80kg. The first power supply of LF is about 25 minutes, the temperature of the molten steel is 1520-1530℃, and the first full component analysis sample is taken. At this time, the refined slag has formed white slag, and the slag composition is CaO: 56±2wt%, SiO2≤6wt%, Al2O3: 27-29wt%, MgO≤5wt%, FeO≤0.5wt%, and the slag basicity R: 7-9.
[0052] At this time, the slag has strong arc burying, air isolation, desulfurization and inclusion absorption capabilities. At this time, the inclusions are mainly MgO-Al2O3 with a size of less than 10μm, and the Ca content in the inclusions is less than 5%; but some CaO-MgO-Al2O3 inclusions with a size of about 15μm and a small amount of Ca are also found.
[0053] After the first full analysis sample is reported, the alloy is fine-tuned according to the composition, and the alloy composition and molten steel temperature are adjusted to the process requirements. After the LF is powered on for the first time, the argon gas flow rate is controlled at 100NL / min, and 50kg of high-purity SiC is used for diffusion deoxidation. At this time, the main task is to maintain the white slag. After the temperature and composition meet the departure requirements, the station will leave and enter the RH.
[0054] LF final slag composition, CaO: 55±2wt%, SiO2≤7wt%, Al2O3: 28~30wt%, MgO≤5wt%,
[0055] FeO≤0.5wt%, slag basicity R: 7~9.
[0056] After LF is completed, no composition adjustment or temperature adjustment is performed to avoid secondary contamination of molten steel. Before LF leaves the station, the inclusions are mainly irregular MgO-Al2O3 with low Ca content and less than 7μm, and the Ca content of the inclusions is less than 5%.
[0057] During RH refining:
[0058] The ladle enters the RH position, argon is connected, the ladle is lifted and vacuum is started, the circulation flow rate is set to 1800NL / min, the mode is selected to be automatic, and the vacuum degree is maintained for 20 minutes after ≤67Pa. At this time, the inclusions are mainly MgO-Al2O3 and Al2O3 inclusions below 6μm, which are most easily removed in the RH process. The circulation flow rate is switched to 1200NL / min and maintained for 10 minutes before breaking the air. During RH re-pressure, the inclusion sizes are mainly MgO-Al2O3 and Al2O3 inclusions of about 5μm.
[0059] After breaking the air, add 6kg of carbonized rice husks to the argon position on the slag surface, start blowing argon from the bottom of the ladle, and start soft blowing. At the beginning of soft blowing, the argon flow rate of the first permeable brick is adjusted to 20NL / min. At this time, the size of inclusions is all MgO-Al2O3 and Al2O3 inclusions ≤5μm. The argon flow rate of the second permeable brick is adjusted to 60NL / min. After 10 minutes of soft blowing, the argon flow rate of the first permeable brick is adjusted to 60NL / min, and the argon flow rate of the second permeable brick is adjusted to 20NL / min. After 10 minutes of soft blowing, continuous casting is performed on the ladle. At this time, the size of inclusions is all MgO-Al2O3 and Al2O3 inclusions ≤3μm.
[0060] CC bloom continuous casting process:
[0061] After the ladle sits on the continuous casting turret, it moves to the pouring position and starts pouring:
[0062] The first step is to put an asbestos water inlet sealing gasket on the ladle outlet. The function of the sealing gasket is to seal the gap between the middle ladle outlet and the large ladle long water inlet to prevent air intake.
[0063] In the second step, the tundish is closed and baked, and the argon tube is inserted into the tundish for argon purging. The purpose of argon purging in the tundish is to clean the air in the tundish and reduce secondary oxidation in the tundish when pouring.
[0064] Put on the big bag long nozzle and insert the argon tube into the long nozzle bowl. Pressurize the air pipe to let argon gas pass through it. The argon flow rate is 20-40NL / min. The purpose of blowing argon gas into the long nozzle bowl is to protect the long nozzle bowl area with inert gas to prevent the long nozzle bowl from inhaling air and causing secondary oxidation.
[0065] After the tundish car is aligned, open the water outlet of the large ladle to inject the molten steel into the tundish. When the water outlet of the large ladle is opened, the ladle drainage sand is taken out. When the molten steel in the tundish reaches 1 / 3 of the tundish volume, close the tundish to fill with argon, and start adding 200kg of high-alkalinity tundish covering agent into the tundish. When the molten steel in the tundish reaches the working liquid level, add 25kg of carbonized rice husk. The main components of the high-alkalinity tundish covering agent are CaO: 45-55wt%, SiO2≥5wt%, Al2O3: 30-35wt%. The high-alkalinity tundish covering agent has a strong adsorption effect on the inclusions in the molten steel in the tundish during the pouring process.
[0066] At this time, the inclusions are mainly MgO-Al2O3 and Al2O3 inclusions with a size of about 2μm. The secondary oxidation of continuous casting and conventional covering agents are a polluting process for molten steel. The inclusion results produced by this method show that the continuous casting process reduces secondary oxidation and does not cause secondary pollution to the molten steel. On the contrary, it has a positive contribution to improving purity.
[0067] Example 2
[0068] This embodiment provides a method for producing bearing steel by adopting an electric furnace-slag removal-LF-RH-CC process.
[0069] The chemical composition of the bearing steel in this embodiment includes, by weight percentage: C: 0.95-1.05%, Si: 0.15-0.35%, Mn: 0.25-0.45%, Cr: 1.40-1.65%, Al: 0.012-0.020wt%, and the rest is Fe and unavoidable impurities.
[0070] The specific process flow of this embodiment is EAF electric furnace smelting → electric furnace slag removal → LF refining → RH refining → CC large square billet continuous casting, wherein:
[0071] During EAF electric furnace smelting:
[0072] The electric furnace adopts a ratio of 95wt% molten iron and 5wt% scrap steel, and adopts the operation of retaining steel and slag. After adding the materials, it adopts the full oxygen blowing smelting method for blowing. After all the scrap steel is melted, lime is added in batches for slag making and dephosphorization.
[0073] In the dephosphorization operation, 1.0 ton of lime is added per 100 tons of steel at the end of the melting period, and automatic slag flow begins. After full melting, according to the amount of slag in the furnace and the requirements of the process for phosphorus in steel, appropriate amount of lime is added, and the amount added each time shall not exceed 500kg per 100 tons of steel.
[0074] When a molten pool is formed in the furnace, carbon is sprayed from the furnace door carbon-oxygen gun to form foamed slag. The amount of carbon powder sprayed is controlled at 5-50 kg / min according to the foamed slag situation.
[0075] When the furnace is fully melted, the temperature is measured. If the temperature is ≥1580℃, a sample is taken for full analysis. At this time, the C content in the steel is 1.0-2.0wt%, and the P content is 0.020-0.035wt%. After the composition is reported, lime is added and oxygen is blown according to the C and P components. The sample is analyzed. At this time, the C content is 0.40-0.70wt%, and the P content is ≤0.015wt%. The temperature is 1630-1640℃. The steel can be tapped if the composition and temperature are qualified.
[0076] The order of deoxidation and alloying of steel is: add 0.8kg / ton of aluminum ingot to 1 / 5 of the steel, add alloy to 1 / 3 of the steel and increase carbon at the same time, and add lime and fluorite to 1 / 2 of the steel.
[0077] During the steel-discharging process, the argon flow rate of the ladle bottom is controlled at 700NL / min. After the steel is discharged, the argon flow rate of the ladle bottom remains unchanged until the ladle receiving position, and the argon flow rate of the ladle bottom is reduced to 400NL / min, and the argon flow rate remains unchanged until the ladle enters the slag removal process.
[0078] During the slagging process after the electric furnace:
[0079] The ladle enters the slag removal position, the argon flow rate is adjusted to about 300mm argon diameter on the slag surface, the ladle is tilted to the specified position, and slag removal begins. The slag in the middle of the slag surface of the ladle is mainly removed. As the slag in the middle is removed, the surrounding slag is gradually blown to the middle of the ladle by the argon gas, and then the slag in the middle is continued to be removed. This reciprocating operation is repeated until the residual slag on the steel liquid surface is less than 100mm in diameter, and the slag removal rate is >97%. The argon gas is turned off and the ladle is transferred to the LF refining receiving position.
[0080] During LF refining:
[0081] The ladle enters the LF refining position, argon is connected, synthetic slag and lime are added, and power is supplied for about 3 minutes. After the slag is melted, high-purity SiC is added for diffusion deoxidation.
[0082] The argon flow rate of the first power supply of LF refining is controlled at 500NL / min, and the amount of diffused deoxidized SiC is 100kg. The first power supply of LF lasts about 25 minutes, the temperature of the molten steel is 1520-1530℃, and the first full component analysis sample is taken. At this time, the refined slag has formed white slag, and the slag composition is CaO: 56±2wt%, SiO2≤6wt%, Al2O3: 27-29wt%, MgO≤5wt%, FeO≤0.5wt%, and the slag basicity R: 7-9.
[0083] At this time, the slag has strong arc burying, air isolation, desulfurization and inclusion absorption capabilities. At this time, the inclusions are mainly MgO-Al2O3 with a size of less than 10μm, and the Ca content in the inclusions is less than 5%; but some CaO-MgO-Al2O3 inclusions with a size of about 15μm and a small amount of Ca are also found.
[0084] After the first full analysis sample is reported, the alloy is fine-tuned according to the composition, and the alloy composition and molten steel temperature are adjusted to the process requirements. After the LF is powered on for the first time, the argon gas flow rate is controlled at 250NL / min, and 50kg of high-purity SiC is used for diffusion deoxidation. At this time, the main task is to maintain the white slag. After the temperature and composition meet the departure requirements, it leaves the station and enters the RH.
[0085] LF final slag composition, CaO: 55±2wt%, SiO2≤7wt%, Al2O3: 28~30wt%, MgO≤5wt%,
[0086] FeO≤0.5wt%, slag basicity R: 7~9.
[0087] After LF is completed, no composition adjustment or temperature adjustment is performed to avoid secondary contamination of molten steel. Before LF leaves the station, the inclusions are mainly irregular MgO-Al2O3 with low Ca content and less than 7μm, and the Ca content of the inclusions is less than 5%.
[0088] During RH refining:
[0089] The ladle enters the RH position, argon is connected, the ladle is lifted and vacuum is started, the circulation flow rate is set to 1800NL / min, the mode is selected to be automatic, and the vacuum degree is maintained for 20 minutes after ≤67Pa. At this time, the inclusions are mainly MgO-Al2O3 and Al2O3 inclusions below 6μm, which are most easily removed in the RH process. The circulation flow rate is switched to 1200NL / min and maintained for 10 minutes before breaking the air. During RH re-pressure, the inclusion sizes are mainly MgO-Al2O3 and Al2O3 inclusions of about 5μm.
[0090] After breaking the air, add 12kg of carbonized rice husks to the argon position on the slag surface, start blowing argon from the bottom of the ladle, and start soft blowing. At the beginning of soft blowing, the argon flow rate of the first permeable brick is adjusted to 40NL / min. At this time, the size of inclusions is all MgO-Al2O3 and Al2O3 inclusions ≤5μm. The argon flow rate of the second permeable brick is adjusted to 80NL / min. After 10 minutes of soft blowing, the argon flow rate of the first permeable brick is adjusted to 80NL / min, and the argon flow rate of the second permeable brick is adjusted to 40NL / min. After 5 minutes of soft blowing, continuous casting is carried out on the ladle. At this time, the size of inclusions is all MgO-Al2O3 and Al2O3 inclusions ≤3μm.
[0091] CC bloom continuous casting process:
[0092] After the ladle sits on the continuous casting turret, it moves to the pouring position and starts pouring:
[0093] The first step is to put an asbestos water inlet sealing gasket on the ladle outlet. The function of the sealing gasket is to seal the gap between the middle ladle outlet and the large ladle long water inlet to prevent air intake.
[0094] In the second step, the tundish is closed and baked, and the argon tube is inserted into the tundish for argon purging. The purpose of argon purging in the tundish is to clean the air in the tundish and reduce secondary oxidation in the tundish when pouring.
[0095] Put on the big bag long nozzle and insert the argon tube into the long nozzle bowl. Pressurize the air pipe to let argon gas pass through it. The argon flow rate is 20-40NL / min. The purpose of blowing argon gas into the long nozzle bowl is to protect the long nozzle bowl area with inert gas to prevent the long nozzle bowl from inhaling air and causing secondary oxidation.
[0096] After the tundish car is aligned, open the water outlet of the large ladle to inject the molten steel into the tundish. When the water outlet of the large ladle is opened, the ladle drainage sand is taken out. When the molten steel in the tundish reaches 1 / 3 of the tundish volume, close the tundish to fill with argon, and start adding 300kg of high-alkalinity tundish covering agent into the tundish. When the molten steel in the tundish reaches the working liquid level, add 35kg of carbonized rice husk. The main components of the high-alkalinity tundish covering agent are CaO: 45-55wt%, SiO2≥5wt%, Al2O3: 30-35wt%. The high-alkalinity tundish covering agent has a strong adsorption effect on the inclusions in the molten steel in the tundish during the pouring process.
[0097] At this time, the inclusions are mainly MgO-Al2O3 and Al2O3 inclusions with a size of about 2μm. The secondary oxidation of continuous casting and conventional covering agents are a polluting process for molten steel. The inclusion results produced by this method show that the continuous casting process reduces secondary oxidation and does not cause secondary pollution to the molten steel. On the contrary, it has a positive contribution to improving purity.
Claims
1. A method for producing bearing steel using an electric furnace-slag removal-LF-RH-CC process, characterized in that: The specific process includes EAF electric furnace smelting → electric furnace slag removal → LF refining → RH refining → CC large square billet continuous casting, among which: During EAF electric furnace smelting: The proportion of 85-95wt% molten iron and 5-15wt% scrap steel is adopted, and the smelting is carried out by full oxygen blowing. After all the scrap steel is melted, lime is added in batches for slagging and dephosphorization, and automatic slag retention is started; when a molten pool is formed in the furnace, carbon oxygen guns at the furnace door are used to spray carbon to form foam slag; after the furnace is fully melted, the temperature is measured and samples are taken, lime is added according to the C and P components, oxygen is blown, and sampling is performed. When the carbon content is 0.30-0.70wt%, P≤0.015wt%, and the temperature is 1610-1640°C, steel is tapped; Deoxidation and alloying of steel are carried out and the argon flow rate of the ladle bottom is controlled. After steel is discharged, the argon flow rate of the ladle bottom remains unchanged until the ladle receiving position, and the argon flow rate of the ladle bottom is reduced until the slag removal process begins; During the slagging process after the electric furnace: The ladle enters the slag removal position, the argon flow rate is adjusted to the argon diameter of the slag surface 300±10mm, the ladle is tilted to the specified position to start slag removal, and the slag removal is completed when the residual slag on the molten steel surface is less than 100mm in diameter, the argon is turned off, and the ladle is transferred to the LF refining ladle receiving position; During LF refining: The ladle enters the LF refining position, argon is connected, synthetic slag and lime are added, and the slag is melted. 80-100kg / 100 tons of steel SiC is added for diffusion deoxidation during the first power supply. The power supply is 25-30 minutes. The temperature of the molten steel is 1520-1530℃. The refined slag forms white slag. The first full component analysis sample is taken. After the analysis sample is reported, the alloy is fine-tuned according to the composition. The alloy composition and molten steel temperature are adjusted to the process requirements. After the first power supply, 30-50kg / 100 tons of steel SiC is added for diffusion deoxidation. The white slag is maintained. After the temperature and composition meet the requirements of leaving the station, the station leaves and enters the RH; During RH refining: The ladle enters the RH position, the argon is turned on, the ladle is lifted and vacuum is started, the circulation flow rate is set to 1800NL / min, and the vacuum degree is maintained for 20-30 minutes after ≤67Pa, and then the circulation flow rate is switched to 1200NL / min and maintained for 10 minutes before breaking the air. After breaking the air, carbonized rice husk is added to start soft blowing. The argon flow rate of the first air brick is 20-40NL / min, and the argon flow rate of the second air brick is 60-80NL / min. After 10 minutes of soft blowing, the argon flow rate of the first air brick is adjusted to 60-80NL / min, and the argon flow rate of the second air brick is adjusted to 20-40NL / min. After 5-10 minutes of soft blowing, continuous casting is carried out on the ladle; CC bloom continuous casting process: After the tundish car is aligned, open the water outlet of the large ladle to inject molten steel into the tundish. When the water outlet of the large ladle is opened, the ladle drainage sand is taken out. When the molten steel in the tundish reaches 1 / 3 of the tundish volume, close the argon flushing of the tundish, and start adding 200-300kg / 100 tons of steel of high alkalinity tundish covering agent into the tundish. After the molten steel in the tundish reaches the working liquid level, add 25-35kg / 100 tons of steel of carbonized rice husk.
2. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 1, characterized in that: During the EAF electric furnace smelting process, slag dephosphorization is carried out by adding 0.8 to 1.0 ton of lime per 100 tons of steel at the end of the melting period. After full melting, no lime is added according to the slag volume in the furnace and the process requirements for phosphorus in steelmaking. The amount of lime added each time shall not exceed 500 kg per 100 tons of steel.
3. A method for producing bearing steel using an electric furnace-slag removal-LF-RH-CC process according to claim 1 or 2, characterized in that: During the EAF electric furnace smelting process, the order of steel deoxidation and alloying is to add 0.8kg / ton of aluminum ingots when 1 / 5 of the steel is tapped, add alloy and increase carbon at the same time when 1 / 3 of the steel is tapped, and add lime and fluorite when 1 / 2 of the steel is tapped.
4. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 3, characterized in that: During the EAF electric furnace smelting process, the argon gas flow rate at the bottom of the ladle during the steel tapping process is 700NL / min, and the argon gas flow rate at the bottom of the ladle at the receiving position is 300-400NL / min.
5. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 4, characterized in that: During the slag removal process at the back of the electric furnace, the slag in the middle of the slag surface of the ladle is mainly removed. As the slag in the middle is removed, the surrounding slag is gradually blown to the middle of the ladle by argon gas, and then the slag in the middle continues to be removed, and the operation is repeated.
6. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 5, characterized in that: During the LF refining process, the argon flow rate is controlled at 300-500 NL / min during the first power supply, and the argon flow rate is controlled at 100-250 NL / min after the first power supply.
7. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 6, characterized in that: During the LF refining process, the final white slag composition is CaO: 55±2wt%, SiO2≤7wt%, Al2O3: 28~30wt%, MgO≤5wt%, FeO≤0.5wt%, and slag basicity R: 7~9.
8. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 7, characterized in that: During the RH refining process, after breaking the air, 6 to 12 kg / 100 tons of steel of carbonized rice husk is added to the argon position on the slag surface, and argon is blown from the bottom of the ladle for soft blowing.
9. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 8, characterized in that: During the continuous casting of CC large square billets, the main components of the high-basicity tundish covering agent are CaO: 45-55wt%, SiO2≥5wt%, and Al2O3: 30-35wt%.
10. The method for producing bearing steel by using electric furnace-slag removal-LF-RH-CC process according to claim 9, characterized in that: The chemical composition of the bearing steel includes, by weight percentage: C: 0.95-1.05%, Si: 0.15-0.35%, Mn: 0.25-0.45%, Cr: 1.40-1.65%, and the rest is Fe and unavoidable impurities.
Citation Information
Cited By
Slagging-off low-alkalinity molten steel smelting method for double-roller thin-strip high-carbon steel
CN122428195A
A method for smelting high-carbon steel with slagging low basicity molten steel by twin-roller thin strip casting
CN122428195B
Method for smelting high-carbon gcr15 steel having low oxygen content and low inclusion content
WO2026207965A1