Biomass carbon preparation process

By carboxylating straw biochar and grafting it with nano-Al2O3 iron oxyhydroxide and graphene oxide, a biomass carbon loaded with graphene oxide is formed, which solves the problem of low stability and low photocatalytic efficiency of biomass carbon under high temperature and strong acid conditions. problem, achieving efficient adsorption and removal of organic pollutants, and is suitable for coal chemical industry and wastewater treatment.

CN118851157AActive Publication Date: 2024-10-29ZHENXIN GREEN SOURCE TECHNOLOGY (FOSHAN) CO LTD

Patent Information

Application Number
CN202411355278.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-10-29
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

Existing biomass carbon has insufficient stability under high temperature and strong acid conditions, has low photocatalytic oxidative degradation efficiency, and is difficult to effectively adsorb and remove organic pollutants in water.

Method used

By carboxylating straw biochar and reacting and grafting it with iron oxyhydroxide and graphene oxide coated with nano-Al2O3 on the surface, a biomass carbon material loaded with graphene oxide is formed, which improves its acid resistance, high temperature resistance and light resistance. Catalytic oxidative degradation rate.

Benefits of technology

It improves the adsorption and removal capacity of biomass carbon for organic pollutants, enhances its environmental protection and photocatalytic efficiency, can work stably under high temperature and strong acid conditions, reduces carbon dioxide emissions, and is suitable for the fields of coal chemical industry and wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a biomass carbon preparation process, and relates to the technical field of biomass carbon preparation, and the biomass carbon is obtained by performing low-temperature carbonization on biomass such as crop straw, performing carboxylation modification, and performing reaction grafting on the biomass, iron oxyhydroxide with the surface coated with nano Al2O3 and graphene oxide. The biomass carbon disclosed by the invention can be applied to the field of coal chemical industry, replaces coal to be used in preparation of synthesis gas, and has an extremely high advantage in the aspect of reducing carbon dioxide emission. The biomass carbon disclosed by the invention has excellent adsorption and removal performance on organic pollutants, and is good in acid resistance and high temperature resistance and high in environmental protection property. Therefore, the biomass carbon disclosed by the invention is widely applied to the fields of coal chemical industry and wastewater treatment, provides possibility for diversified utilization of biomass, and is worthy of popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomass carbon preparation, and in particular to a biomass carbon preparation process. Background Art

[0002] Biomass carbon refers to a carbon-rich material with a high degree of aromatization and a large specific surface area produced by biomass materials such as sludge, animal manure and plant residues under anaerobic or anoxic conditions and a certain pyrolysis temperature. Synthesis gas is a raw gas with carbon monoxide and hydrogen as the main components and is used as a chemical raw material. The raw materials for synthesis gas are very wide. It can be produced by gasification of solid fuels such as coal or coke, or by light hydrocarbons such as natural gas and naphtha, or by partial oxidation of heavy oil. Coal and other materials have disadvantages such as high carbon dioxide emissions in the preparation process of synthesis gas, which is not conducive to environmental protection. How to use biomass carbon in the preparation of synthesis gas, reduce carbon dioxide emissions, and improve environmental protection is worthy of in-depth study.

[0003] Since biomass carbon contains abundant oxygen-containing functional groups and large porosity, it has good adsorption and stabilization effects on pollutants present in the ecological environment (water, soil or sediment). Iron oxyhydroxide (FeOOH) is a semiconductor material with excellent performance. Under the action of sunlight, it can be used as a photocatalyst to oxidize and degrade organic matter in wastewater to generate H 2 O and CO 2 However, ferric hydroxide is easily decomposed under high temperature and strong acid conditions, resulting in insufficient stability. In addition, the photon efficiency of ferric hydroxide is relatively low, which makes its effective utilization rate of light energy insufficient, and has an adverse effect on its photocatalytic oxidation degradation rate. Therefore, a biomass carbon material combining ferric hydroxide with biomass carbon is developed, so that the acid resistance, high temperature resistance and photocatalytic oxidation degradation reaction rate of the biomass carbon material can be improved, thereby having a better adsorption and removal ability for organic matter in wastewater, which has practical significance. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a biomass carbon preparation process.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] The biomass carbon is prepared by the following steps:

[0007] Step S1: Wash the straw, dry it and crush it, heat it to 400-500°C in a protective gas atmosphere, keep it at a constant temperature for 5-6 hours, then take it out, grind and sieve it to obtain raw biochar; add the raw biochar to a nitric acid solution, heat it at 90-100°C for 10-12 hours, cool it to room temperature, wash it to neutrality, and vacuum dry it at 80-90°C for 3-4 hours to obtain a carboxylated biochar material;

[0008] Furthermore, the straw is crop straw, the protective gas is nitrogen, the mesh number used for sieving is 100 meshes; the dosage ratio of the original biochar and the nitric acid solution is 1g:40-50mL, and the mass fraction of the nitric acid solution is 68-70%.

[0009] In the reaction process of step S1, the straw is carbonized at high temperature to obtain raw biochar; the raw biochar is acidified with nitric acid solution to obtain carboxylated biochar material;

[0010] Step S2: Add ferric hydroxide to deionized water, ultrasonically disperse for 30-40 minutes, then add sodium hexametaphosphate, adjust the pH to 8-9, heat to 80-90°C under stirring, adjust the pH to 10.0-10.8, add hydrated aluminum oxide, continue stirring for 0.5-1h, adjust the pH to 7.0, continue stirring for 20-40 minutes, filter, wash with water, and dry to obtain the surface-coated nano-Al 2 O 3 of iron oxyhydroxide;

[0011] Further, the dosage ratio of ferric oxyhydroxide, deionized water, sodium hexametaphosphate, and hydrated aluminum oxide is 5-10 g: 50-60 mL: 3-6 g: 0.05-0.1 g, and the ferric oxyhydroxide is δ-FeOOH (the preparation process of δ-FeOOH refers to Item 2.1 of the paper "Preparation of δ-FeOOH and FTIR Spectrum of Heat-treated Product");

[0012] In step S2, the nano-Al 2 O 3 Physical coating on the surface of iron oxyhydroxide;

[0013] Step S3: Coating the surface with nano-Al 2 O 3 Add ethanol to the ferric hydroxide and stir for 30-40 minutes to obtain a ferric hydroxide ethanol solution; then add oleic acid to ethanol and stir for 5-10 minutes, then pour it into the ferric hydroxide ethanol solution, stir and react at 60-70°C for 1-2 hours, dry and grind to obtain a coated product; add the coated product to dichloromethane, stir and add 3-chloroperoxybenzoic acid, stir and react at room temperature for 4-5 hours to obtain an epoxy product;

[0014] Furthermore, the surface is coated with nano-Al 2 O 3The dosage ratio of ferric hydroxide oxide and ethanol is 1g:20-30mL, the dosage ratio of oleic acid, ethanol and ferric hydroxide oxide ethanol solution is 5-6mL:30-40mL:30-40mL, and the volume fraction of ethanol is 95%; the dosage ratio of coated product, dichloromethane and 3-chloroperoxybenzoic acid is 10-12g:100-110mL:36-40g;

[0015] During the reaction of step S3, oleic acid is used to coat the surface of nano-Al 2 O 3 The ferric hydroxide is wet-modified to generate a coating product with unsaturated double bonds on the surface; the unsaturated double bonds of the coating product are oxidized by 3-chloroperoxybenzoic acid to generate an epoxy product;

[0016] Step S4: In a protective gas atmosphere, the carboxylated biochar material and toluene are mixed and heated to 40-50°C, pyridine is added, stirred, the epoxy product is added, stirred and reacted for 8-10 hours, and then the temperature is raised to 110-120°C, stirred for 1-2 hours, to obtain a hydroxyl product;

[0017] Further, the protective gas is nitrogen, and the usage ratio of the carboxylated biochar material, toluene, pyridine and epoxidation product is 32-35 g: 140-150 mL: 0.5-0.6 mol: 21-23 g;

[0018] During the reaction process of step S4, the carboxyl group of the carboxylated biochar material reacts with the epoxy group of the epoxy product to coat the surface with nano-Al 2 O 3 The iron oxyhydroxide is loaded in biochar to obtain hydroxyl products;

[0019] Step S5: adding graphene oxide to DMF, adding thionyl chloride with stirring, reflux stirring and reacting for 24-26 hours to obtain an acyl chloride product; mixing the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to obtain a mixed solution 1; adding the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2, adding the mixed solution 2 dropwise to the mixed solution 1 in an ice water bath, and after the addition is complete, heating to 70-80° C., stirring at a constant temperature for 8-10 hours, and then heating to 100-110° C., continuing to stir for 1-2 hours, and distilling under reduced pressure to obtain biomass carbon;

[0020] Further, the usage ratio of graphene oxide, DMF, and dichlorothionyl is 5-6 g: 55-65 mL: 15-20 g; the usage ratio of hydroxyl product, pyridine, triethylamine, and dimethyl sulfoxide is 10-12 g: 0.02-0.03 mol: 0.1 mol: 80-90 mL; the usage ratio of acyl chloride product and dimethyl sulfoxide is 8-10 g: 60-70 mL; the usage ratio of mixed solution 1 and mixed solution 2 is 85-95 mL: 65-75 mL;

[0021] In the reaction process of step S5, graphene oxide reacts with thionyl chloride to generate an acyl chloride product, and the acyl chloride product then undergoes an esterification reaction with a hydroxyl product to obtain a loaded graphene oxide and a surface-coated nano-Al 2 O 3 of iron oxyhydroxide on biomass carbon.

[0022] Beneficial effects of the invention: The invention discloses a biomass carbon preparation process, wherein the biomass carbon is obtained by carboxylating straw biochar and coating it with nano-Al 2 O 3 The biomass carbon obtained by the reaction modification of the straw biochar can be mixed with water to form a uniform slurry with a mass fraction of 60-63%. The slurry is placed in a gasifier for more complete gasification, and can replace coal for the preparation of synthesis gas. In addition, in the process of preparing synthesis gas with biomass carbon, carbon dioxide emissions are reduced, which is very beneficial to environmental protection.

[0023] Compared with ordinary crop straw biochar, biochar has enhanced adsorption capacity for organic pollutants in water due to the loading of iron oxyhydroxide and graphene oxide; 2 O 3 After coating, the acid resistance and high temperature resistance of ferric oxyhydroxide are improved because nano-alumina has strong acid resistance and excellent thermal stability. 2 O 3 The ferric oxyhydroxide is not easy to agglomerate but is evenly dispersed. The ferric oxyhydroxide can absorb sunlight and photocatalytically oxidize and degrade the adsorbed organic pollutants into non-toxic H 2 O and CO 2 , In addition, δ-FeOOH has magnetism, so that the biomass carbon obtained can be collected by magnetic adsorption, avoiding the adverse effects of biomass carbon on the environment due to its light weight, small particles and difficulty in separation, and improving the environmental friendliness of biomass carbon; Graphene oxide has the advantages of photosensitivity, good conductivity, and high carrier mobility. It is grafted with hydroxyl iron semiconductor materials and loaded in biomass carbon, and the agglomeration phenomenon of graphene oxide is also improved. At the same time, the migration rate of electrons in biomass carbon can be increased, the recombination time of electron-hole pairs can be reduced, the photocatalytic efficiency of hydroxyl iron can be enhanced, and the deficiency of low photoquantum efficiency of hydroxyl iron can be compensated, so that organic pollutants can be quickly adsorbed and removed. Therefore, the biomass carbon prepared by the present invention has strong adsorption and removal capabilities for organic pollutants, and has good high temperature resistance and acid resistance, high environmental protection, and is worthy of promotion.

[0024] Therefore, the biochar of the present invention can be applied not only to the field of coal chemical industry, but also to the field of wastewater treatment, which is very beneficial for realizing the diversified utilization of biomass materials. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] A biomass carbon, the preparation of which comprises the following steps:

[0028] Step S1: Wash and dry the rice straw and then crush it, heat it to 400°C in a nitrogen atmosphere, keep it at a constant temperature for 5 hours, then take it out and grind it through a 100-mesh sieve to obtain raw biochar; add the raw biochar to a nitric acid solution, heat it at 90°C for 10 hours, cool it to room temperature, wash it to neutrality, and vacuum dry it at 80°C for 3 hours to obtain a carboxylated biochar material; the dosage ratio of the raw biochar to the nitric acid solution is 1g:40mL, and the mass fraction of the nitric acid solution is 68%.

[0029] Step S2: Add ferric hydroxide to deionized water, ultrasonically disperse for 30 minutes, then add sodium hexametaphosphate, adjust the pH to 8, heat to 80°C under stirring, adjust the pH to 10.0, add hydrated aluminum oxide, continue stirring for 0.5h, adjust the pH to 7.0, continue stirring for 20min, filter, wash with water, and dry to obtain the surface-coated nano-Al 2 O 3 The amount ratio of ferric oxyhydroxide, deionized water, sodium hexametaphosphate and hydrated alumina is 5g:50mL:3g:0.05g, and the ferric oxyhydroxide is δ-FeOOH (the preparation process of δ-FeOOH refers to the content of 2.1 of the paper "Preparation of δ-FeOOH and FTIR Spectrum of Heat Treatment Product");

[0030] Step S3: Coating the surface with nano-Al 2 O 3 The ferric hydroxide was added with ethanol and stirred for 30 minutes to obtain a ferric hydroxide ethanol solution; oleic acid was added with ethanol and stirred for 5 minutes, then poured into the ferric hydroxide ethanol solution, stirred and reacted at 60°C for 1 hour, dried and ground to obtain a coated product; the coated product was added into dichloromethane, 3-chloroperoxybenzoic acid was added and stirred, and the reaction was stirred at room temperature for 4 hours to obtain an epoxy product; the surface was coated with nano-Al 2 O 3The dosage ratio of ferric hydroxide oxide and ethanol is 1g:20mL, the dosage ratio of oleic acid, ethanol and ferric hydroxide oxide ethanol solution is 5mL:30mL:30mL, and the volume fraction of ethanol is 95%; the dosage ratio of coated product, dichloromethane and 3-chloroperoxybenzoic acid is 10g:100mL:36g;

[0031] Step S4: In a nitrogen atmosphere, the carboxylated biochar material and toluene are mixed and heated to 40°C, pyridine is added, stirred, the epoxy product is added, stirred and reacted for 8 hours, and then the temperature is raised to 110°C and stirred for 1 hour to obtain a hydroxyl product; the amount ratio of the carboxylated biochar material, toluene, pyridine and epoxy product is 32g:140mL:0.5mol:21g;

[0032] Step S5: adding graphene oxide to DMF, adding dichlorothionyl with stirring, reflux stirring and reacting for 24 hours to obtain an acyl chloride product; mixing the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to obtain a mixed solution 1; adding the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2, adding the mixed solution 2 dropwise to the mixed solution 1 in an ice-water bath, heating to 70°C after the addition is complete, stirring at a constant temperature for 8 hours, and then heating to 100°C, continuing to stir for 1 hour, and distilling under reduced pressure to obtain biomass carbon; the amount ratio of graphene oxide, DMF, and dichlorothionyl is 5g:55mL:15g; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 10g:0.02mol:0.1mol:80mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 8g:60mL; the amount ratio of the mixed solution 1 to the mixed solution 2 is 85mL:65mL.

[0033] Example 2

[0034] A biomass carbon, the preparation of which comprises the following steps:

[0035] Step S1: Wash and dry the corn stalks and crush them, heat them to 450°C in a nitrogen atmosphere, keep the constant temperature for 5.5 hours, take them out, grind them through a 100-mesh sieve to obtain raw biochar; add the raw biochar to a nitric acid solution, heat it at 95°C for 11 hours, cool it to room temperature, wash it to neutrality, and vacuum dry it at 85°C for 3.5 hours to obtain a carboxylated biochar material; the dosage ratio of the raw biochar to the nitric acid solution is 1g:45mL, and the mass fraction of the nitric acid solution is 69%.

[0036] Step S2: Add ferric hydroxide to deionized water, ultrasonically disperse for 35 minutes, then add sodium hexametaphosphate, adjust the pH to 8, heat to 85°C under stirring, adjust the pH to 10.4, add hydrated aluminum oxide, continue stirring for 0.8 hours, adjust the pH to 7.0, continue stirring for 30 minutes, filter, wash with water, and dry to obtain the surface-coated nano-Al 2 O 3The amount ratio of ferric oxyhydroxide, deionized water, sodium hexametaphosphate and hydrated alumina is 8g:55mL:4.5g:0.08g, and the ferric oxyhydroxide is δ-FeOOH (the preparation process of δ-FeOOH refers to the content of 2.1 of the paper "Preparation of δ-FeOOH and FTIR Spectrum of Heat Treatment Product");

[0037] Step S3: Coating the surface with nano-Al 2 O 3 The ferric hydroxide was added with ethanol and stirred for 35 minutes to obtain a ferric hydroxide ethanol solution; oleic acid was added with ethanol and stirred for 8 minutes, then poured into the ferric hydroxide ethanol solution, stirred and reacted at 65°C for 1.5 hours, dried and ground to obtain a coated product; the coated product was added into dichloromethane, 3-chloroperoxybenzoic acid was added and stirred, and the reaction was stirred at room temperature for 4.5 hours to obtain an epoxy product; the surface was coated with nano-Al 2 O 3 The dosage ratio of ferric hydroxide oxide and ethanol is 1g:25mL, the dosage ratio of oleic acid, ethanol and ferric hydroxide oxide ethanol solution is 5mL:35mL:35mL, and the volume fraction of ethanol is 95%; the dosage ratio of coated product, dichloromethane and 3-chloroperoxybenzoic acid is 11g:105mL:38g;

[0038] Step S4: In a nitrogen atmosphere, the carboxylated biochar material and toluene are mixed and heated to 45°C, pyridine is added, stirred, the epoxy product is added, stirred and reacted for 9 hours, and then the temperature is raised to 115°C and stirred for 1.5 hours to obtain a hydroxyl product; the amount ratio of the carboxylated biochar material, toluene, pyridine and epoxy product is 33g:145mL:0.5mol:22g;

[0039] Step S5: adding graphene oxide to DMF, adding dichlorothionyl with stirring, reflux stirring and reacting for 25 hours to obtain an acyl chloride product; mixing the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to obtain a mixed solution 1; adding the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2, adding the mixed solution 2 dropwise to the mixed solution 1 in an ice-water bath, heating to 75°C after the addition is complete, stirring at a constant temperature for 9 hours, and then heating to 105°C, continuing to stir for 1.5 hours, and distilling under reduced pressure to obtain biomass carbon; the amount ratio of graphene oxide, DMF, and dichlorothionyl is 5.5g:60mL:18g; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 11g:0.02mol:0.1mol:85mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 9g:65mL; ​​the amount ratio of the mixed solution 1 to the mixed solution 2 is 90mL:70mL.

[0040] Example 3

[0041] A biomass carbon, the preparation of which comprises the following steps:

[0042] Step S1: Wash and dry the Salix psammophila straw and then crush it, heat it to 500°C in a nitrogen atmosphere, keep it at a constant temperature for 6 hours, then take it out and grind it through a 100-mesh sieve to obtain raw biochar; add the raw biochar to a nitric acid solution, heat it at 100°C for 12 hours, then cool it to room temperature, wash it to neutrality, and vacuum dry it at 90°C for 4 hours to obtain a carboxylated biochar material; the dosage ratio of the raw biochar to the nitric acid solution is 1g:50mL, and the mass fraction of the nitric acid solution is 70%.

[0043] Step S2: Add ferric hydroxide to deionized water, ultrasonically disperse for 40 minutes, then add sodium hexametaphosphate, adjust the pH to 9, heat to 90°C under stirring, adjust the pH to 10.8, add hydrated aluminum oxide, continue stirring for 1 hour, adjust the pH to 7.0, continue stirring for 40 minutes, filter, wash with water, and dry to obtain the surface-coated nano-Al 2 O 3 The amount ratio of ferric oxyhydroxide, deionized water, sodium hexametaphosphate and hydrated alumina is 10g:60mL:6g:0.1g, and the ferric oxyhydroxide is δ-FeOOH (the preparation process of δ-FeOOH refers to the content of 2.1 of the paper "Preparation of δ-FeOOH and FTIR Spectrum of Heat Treatment Product");

[0044] Step S3: Coating the surface with nano-Al 2 O 3 The ferric hydroxide was added with ethanol and stirred for 40 minutes to obtain a ferric hydroxide ethanol solution; oleic acid was added with ethanol and stirred for 10 minutes, then poured into the ferric hydroxide ethanol solution, stirred and reacted at 70°C for 2 hours, dried and ground to obtain a coated product; the coated product was added into dichloromethane, 3-chloroperoxybenzoic acid was added and stirred, and the reaction was reacted at room temperature for 5 hours to obtain an epoxy product; the surface was coated with nano-Al 2 O 3 The dosage ratio of ferric hydroxide oxide and ethanol is 1g:30mL, the dosage ratio of oleic acid, ethanol and ferric hydroxide oxide ethanol solution is 6mL:40mL:40mL, and the volume fraction of ethanol is 95%; the dosage ratio of coated product, dichloromethane and 3-chloroperoxybenzoic acid is 12g:110mL:40g;

[0045] Step S4: In a nitrogen atmosphere, the carboxylated biochar material and toluene are mixed and heated to 50°C, pyridine is added, stirred, the epoxy product is added, stirred and reacted for 10 hours, and then the temperature is raised to 120°C and stirred for 2 hours to obtain a hydroxyl product; the amount ratio of the carboxylated biochar material, toluene, pyridine and epoxy product is 35g:150mL:0.6mol:23g;

[0046] Step S5: adding graphene oxide to DMF, adding dichlorothionyl with stirring, reflux stirring and reacting for 26 hours to obtain an acyl chloride product; mixing the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide to obtain a mixed solution 1; adding the acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2, dripping the mixed solution 2 into the mixed solution 1 in an ice water bath, after the dripping is completed, heating to 80°C, stirring at a constant temperature for 10 hours, and then heating to 110°C, continuing to stir for 2 hours, and distilling under reduced pressure to obtain biomass carbon; the amount ratio of graphene oxide, DMF, and dichlorothionyl is 6g:65mL:20g; the amount ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 12g:0.03mol:0.1mol:90mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 10g:70mL; the amount ratio of the mixed solution 1 to the mixed solution 2 is 95mL:75mL.

[0047] Comparative Example 1

[0048] Compared with Example 3, this comparative example is the original biochar obtained in step S1 of Example 3, that is, the biochar without surface-coated nano-Al 2 O 3 Biomass carbon with iron oxyhydroxide and graphene oxide.

[0049] Comparative Example 2

[0050] Compared with Example 3, the surface of step S3 of Example 3 is coated with nano-Al 2 O 3 The ferric oxyhydroxide is replaced by the ferric oxyhydroxide in step S2, that is, the surface of the ferric oxyhydroxide is not coated with nano-alumina, to obtain biomass carbon.

[0051] Comparative Example 3

[0052] Compared with Example 3, this comparative example is the hydroxyl product obtained in step S4 of Example 3, that is, graphene oxide is not introduced, and only the surface-coated nano-Al 2 O 3 of iron oxyhydroxide on biomass carbon.

[0053] The biomass carbon prepared by the present invention is further tested for its effect, and the test results are as follows.

[0054] 60g of each of the coal, the biomass carbon obtained in Examples 1-3 and Comparative Example 1 were added with 40mL of distilled water and stirred to prepare slurry, and then the slurry was placed in a pulverized coal gasifier under the following gasification conditions: gasification temperature 1380°C, gasification pressure 6.5MPa, flux (quartz sand) 12g, oxygen concentration 99.6mol% to prepare synthesis gas, and the gasification performance was tested. The test results are recorded in Table 1:

[0055] Table 1:

[0056]

[0057] According to the data in Table 1, it can be seen from the gasification performance test of the biomass carbon obtained in Examples 1-3 of the present invention and coal that the biomass carbon of the present invention can be used to prepare syngas to obtain a gasification performance similar to that of coal, and it is possible to replace coal for syngas preparation. 2 O 3 The biomass carbon containing iron oxyhydroxide and graphene oxide can be mixed with water to form a more uniform slurry, which is more conducive to the complete combustion of the biomass carbon in the gasifier and obtains better gasification results.

[0058] Fluoranthene, perchloroethylene and 4-chlorophenol were selected as samples for testing. Under certain pH and temperature conditions, sample solutions with an initial concentration of 50 mg / L, namely, fluoranthene solution, perchloroethylene solution and 4-chlorophenol solution, were added to reagent bottles respectively. Then, the biomass carbon obtained in Examples 1-3 and Comparative Examples 1-3 was added to the fluoranthene solution, perchloroethylene solution and 4-chlorophenol solution. After standing for 7 days, the concentrations of the sample solutions, namely, fluoranthene solution, perchloroethylene solution and 4-chlorophenol solution, were measured. The degradation rates of fluoranthene, perchloroethylene and 4-chlorophenol were calculated. The degradation rate (%) = (50-sample solution concentration after 7 days) / 50*100. The results are recorded in Table 2.

[0059] Table 2: Test results

[0060]

[0061] According to the data in Table 2, the biomass carbon prepared by the present invention has excellent adsorption and removal performance for organic pollutants. 2 O 3 The iron oxyhydroxide is less affected by strong acidity and high temperature, so the obtained biomass carbon has good high temperature resistance and acid resistance. 2 O 3 Although the ordinary raw biochar is less affected by strong acidity and high temperature, the degradation rate of organic pollutants is significantly reduced. Therefore, the prepared biomass carbon has better adsorption and removal performance for organic pollutants. 2 O 3 Biomass carbon coated with iron oxyhydroxide and graphene oxide without nano-Al 2 O 3The performance of the coated ferric hydroxide is less affected under normal temperature and neutral conditions, but the acid resistance and high temperature resistance are reduced, so that the adsorption and removal performance of the prepared biomass carbon for organic pollutants under high temperature and strong acid conditions is greatly reduced. 2 O 3 The biomass carbon of iron oxyhydroxide is prepared without introducing graphene oxide to improve the photocatalytic performance of iron oxyhydroxide, which is not conducive to improving the degradation rate of organic pollutants.

[0062] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A biomass carbon preparation process, characterized in that: The steps include: Step S1: Wash the straw, dry it and crush it, heat it to 400-500°C in a protective gas atmosphere, keep it at a constant temperature for 5-6 hours, then take it out, grind and sieve it to obtain raw biochar; add the raw biochar to a nitric acid solution, heat it at 90-100°C for 10-12 hours, cool it to room temperature, wash it to neutrality, and vacuum dry it at 80-90°C for 3-4 hours to obtain a carboxylated biochar material; Step S2: adding oxyhydroxide to deionized water, ultrasonically dispersing for 30-40 minutes, then adding sodium hexametaphosphate, adjusting the pH to 8-9, heating to 80-90° C. with stirring, adjusting the pH to 10.0-10.8, adding hydrated aluminum oxide, continuing stirring for 0.5-1 hour, adjusting the pH to 7.0, continuing stirring for 20-40 minutes, filtering, washing with water, and drying to obtain oxyhydroxide with surface coated with nano-Al2O3; Step S3: adding ethanol to the iron hydroxide with the surface coated with nano-Al2O3 and stirring for 30-40 minutes to obtain an iron hydroxide ethanol solution; then adding oleic acid to ethanol and stirring for 5-10 minutes, and then pouring into the iron hydroxide ethanol solution, stirring and reacting at 60-70°C for 1-2 hours, drying and grinding to obtain a coated product; The coated product was added to dichloromethane, 3-chloroperoxybenzoic acid was added with stirring, and the reaction was stirred at room temperature for 4-5 hours to obtain the epoxy product; Step S4: In a protective gas atmosphere, the carboxylated biochar material and toluene are mixed and heated to 40-50°C, pyridine is added, stirred, the epoxy product is added, stirred and reacted for 8-10 hours, and then the temperature is raised to 110-120°C, stirred for 1-2 hours, to obtain a hydroxyl product; Step S5: adding graphene oxide to DMF, adding thionyl chloride with stirring, and reacting with reflux and stirring for 24-26 hours to obtain an acyl chloride product; The hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide are mixed to obtain a mixed solution 1; the acyl chloride product is added to dimethyl sulfoxide to obtain a mixed solution 2; the mixed solution 2 is added dropwise to the mixed solution 1 in an ice water bath; after the addition is completed, the temperature is raised to 70-80°C, and the reaction is stirred at a constant temperature for 8-10 hours, and then the temperature is raised to 100-110°C, and the stirring is continued for 1-2 hours, and the biomass carbon is obtained by distillation under reduced pressure.

2. A biomass carbon preparation process according to claim 1, characterized in that: In step S1, the straw is crop straw, and the mesh number used for sieving is 100 meshes.

3. A biomass carbon preparation process according to claim 1, characterized in that: In step S1, the dosage ratio of the original biochar and the nitric acid solution is 1 g: 40-50 mL, and the mass fraction of the nitric acid solution is 68-70%.

4. A biomass carbon preparation process according to claim 1, characterized in that: In step S2, the usage ratio of ferric oxyhydroxide, deionized water, sodium hexametaphosphate and hydrated aluminum oxide is 5-10 g: 50-60 mL: 3-6 g: 0.05-0.1 g.

5. A biomass carbon preparation process according to claim 1, characterized in that: In step S3, the usage ratio of ferric hydroxide oxide coated with nano-Al2O3 and ethanol is 1g:20-30mL, the usage ratio of oleic acid, ethanol and ferric hydroxide oxide ethanol solution is 5-6mL:30-40mL:30-40mL, and the volume fraction of ethanol is 95%.

6. A biomass carbon preparation process according to claim 1, characterized in that: In step S3, the usage ratio of the coated product, dichloromethane and 3-chloroperbenzoic acid is 10-12 g: 100-110 mL: 36-40 g.

7. A biomass carbon preparation process according to claim 1, characterized in that: In step S4, the usage ratio of carboxylated biochar material, toluene, pyridine and epoxidation product is 32-35 g: 140-150 mL: 0.5-0.6 mol: 21-23 g.

8. A biomass carbon preparation process according to claim 1, characterized in that: In step S5, the usage ratio of graphene oxide, DMF and thionyl chloride is 5-6 g: 55-65 mL: 15-20 g.

9. A biomass carbon preparation process according to claim 1, characterized in that: In step S5, the usage ratio of the hydroxyl product, pyridine, triethylamine and dimethyl sulfoxide is 10-12 g: 0.02-0.03 mol: 0.1 mol: 80-90 mL; the usage ratio of the acyl chloride product and dimethyl sulfoxide is 8-10 g: 60-70 mL.

10. The biomass carbon preparation process according to claim 1, characterized in that: In step S5, the usage ratio of mixed solution 1 to mixed solution 2 is 85-95 mL:65-75 mL.

Citation Information

Patent Citations

  • Preparation method of heteroatom doped graphene hierarchical pore carbon material

    CN106044754A

  • Fe-Co-RGO (iron-cobalt-reduced graphene oxide) composite wave absorbing material and preparation method thereof

    CN109054742A

  • FeOOH composite material as well as preparation method and application thereof

    CN118403611A

  • Method of preparing iron oxide-graphene composites and the iron oxide(β-FeOOH)-graphene composites prepared by the same method

    KR1020150116489A

Cited By

  • Synthetic method of p-hydroxybenzoic acid

    CN119143594A

  • Energy-saving and environment-friendly furnace top nano heat-preservation castable

    CN119661242A