Preparation process of environment-friendly degradable corrosion-resistant sealing grease
By preparing anti-rust, viscosity adjustment and anti-corrosion additives, combined with biodegradable base oil, the problems of insufficient corrosion resistance and environmental pollution of traditional sealing grease are solved, and a sealing grease with efficient sealing performance and environmental protection properties is achieved.
Patent Information
- Application Number
- CN202410866913.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-01
AI Technical Summary
Traditional sealing grease has insufficient corrosion resistance during use and is prone to oxidation, leading to seal failure and affecting the normal operation and service life of the equipment. It also contains components that are difficult to degrade and cause environmental pollution.
An environmentally friendly degradable corrosion-resistant sealing grease preparation process is used to prepare anti-rust additives by mixing and heating methyl oleate and maleic anhydride; tannic acid, ethyl acetate, butyl acetate, triphenyl Phosphine and hydroquinone Monomethyl ether and other components are mixed to prepare viscosity adjustment additives; n-bromooctane, n-bromodecane and tri-n-butylphosphine are reacted with mercaptobenzothiazole and potassium hydroxide to prepare anti-corrosion additives, which are added to the base oil , forming a sealing grease.
It improves the corrosion resistance and adhesion of sealing grease, extends its service life, reduces environmental pollution, and achieves environmentally friendly and non-toxic effects through biodegradable materials.
Smart Images

Figure CN118853263A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing grease, and in particular to a preparation process of environmentally friendly, degradable and corrosion-resistant sealing grease. Background Art
[0002] Sealing grease is a material mainly used in the tail part of the shield machine to perform sealing and lubrication. It is a uniform paste made from base oil and various additives such as fiber, tackifier, filler, etc.
[0003] While traditional sealing greases provide effective sealing and lubrication, they usually contain ingredients that are difficult to degrade, which can burden the environment after long-term use. In addition, existing sealing greases often lack corrosion resistance and can oxidize during use, especially when exposed to acidic and alkaline media, salt spray environments, or high temperatures. They are prone to performance degradation, leading to sealing failure, and thus affecting the normal operation and service life of the equipment.
[0004] Therefore, we proposed a preparation process of environmentally friendly biodegradable and corrosion-resistant sealing grease to extend the service life of the sealing grease and reduce environmental pollution. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention aims to provide an environmentally friendly, biodegradable, and corrosion-resistant sealing grease, which not only has excellent sealing performance and corrosion resistance, but also can be rapidly degraded in the natural environment to reduce environmental pollution.
[0006] A preparation process of an environmentally friendly biodegradable corrosion-resistant sealing grease comprises the following steps:
[0007] S1: Preparation of anti-rust additives
[0008] Methyl oleate and maleic anhydride are mixed and heated to react, and then distilled under reduced pressure, and then mixed and heated with distilled water to perform a hydrolysis reaction, and then distilled under reduced pressure again to obtain an anti-rust additive;
[0009] S2: Preparation of viscosity-adjusting additives
[0010] Tannic acid, ethyl acetate, butyl acetate, triphenylphosphine and hydroquinone monomethyl ether are stirred and mixed, and glycidyl methacrylate and Versatic acid glycidyl ester are added, and heated to react to obtain a viscosity regulating additive;
[0011] S3: Preparation of anti-corrosion additives
[0012] Uniformly mixing n-octane bromide, n-decane bromide and tri-n-butylphosphine to react and prepare intermediate A, dissolving intermediate A in methanol to form intermediate A solution for later use, then dissolving mercaptobenzothiazole and potassium hydroxide in methanol to prepare a ternary mixed solution for later use, and then adding the intermediate A solution to the ternary mixed solution for reaction to obtain an anticorrosive additive;
[0013] S4: Mix the components to prepare sealing grease
[0014] Add the base oil, the above-mentioned anti-rust additive, the above-mentioned viscosity regulating additive and the above-mentioned anti-corrosion additive into a kneader, knead for 30-40 minutes, then add the grease into the kneader, continue kneading for 40-50 minutes, then add the fiber into the kneader, continue kneading for 20-30 minutes, then add the filler into the kneader, continue kneading for 2-3 hours to obtain the sealing grease.
[0015] Furthermore, S1 specifically includes the following steps:
[0016] S1.1: Add methyl oleate and maleic anhydride in a molar ratio of 1:(1.3-1.8) into a reactor, stir and mix well, heat at 200-260°C for 8-10h to react, and cool naturally to room temperature to obtain a crude product;
[0017] S1.2: placing the crude product in a vacuum distiller, removing impurities by vacuum distillation, and naturally cooling to room temperature to obtain a precursor;
[0018] S1.3: The above precursor and distilled water are stirred and mixed evenly in a molar ratio of 1:(3-5), and then heated at a temperature of 60-80°C for 6-8h to carry out a hydrolysis reaction, and then the excess distilled water is removed by reduced pressure distillation to obtain an anti-rust additive.
[0019] Furthermore, S2 specifically includes the following steps:
[0020] S2.1: Add tannic acid, ethyl acetate and butyl acetate into a reaction tank at a solid-liquid ratio of (15-20) g: (16-20) mL: (7-9) mL, heat at 80-90° C., stir at a rate of 200-300 r / min for 30-40 min, and mix thoroughly to obtain a mixed solution A;
[0021] S2.2: Keep the heating temperature unchanged, adjust the stirring rate to 100-200 r / min, add triphenylphosphine and hydroquinone monomethyl ether to the mixed solution A while stirring, and continue stirring for 20-30 min to obtain a mixed solution B;
[0022] S2.3: Keeping the heating temperature and stirring rate unchanged, add glycidyl methacrylate and glycidyl versatic acid to the mixed solution B while stirring, heat the reaction for 10-12 hours, and remove the solvent by vacuum distillation to obtain a viscosity regulating additive.
[0023] Furthermore, S3 specifically includes the following steps:
[0024] S3.1: n-octane bromide, n-decane bromide and tri-n-butylphosphine are stirred and mixed uniformly in a mass ratio of 1:(1.2-1.4):(1-1.2), and then heated at 140-150° C. for 10-12 h under nitrogen protection to reflux reaction, and impurities are removed by reduced pressure distillation to obtain intermediate A;
[0025] S3.2: Add the intermediate A to methanol at a mass ratio of 1:(60-70), stir thoroughly to dissolve, and obtain an intermediate A solution;
[0026] S3.3: Add mercaptobenzothiazole and potassium hydroxide to methanol at a solid-liquid ratio of (3-5) g: 1 g: (20-30) mL, stir thoroughly to dissolve, and obtain a ternary mixed solution;
[0027] S3.4: adding the intermediate A solution to the ternary mixed solution, and then stirring at a rate of 400-500 r / min for 2-3 hours to react to obtain a suspension, wherein the molar ratio of mercaptobenzothiazole to intermediate A is 1:(1-1.4);
[0028] S3.5: Place the above suspension in a centrifuge and perform centrifugal filtration to remove solid impurities, then perform rotary evaporation on the filtrate to remove the solvent and water to obtain intermediate B;
[0029] S3.6: Add the intermediate B mentioned above to anhydrous ethanol, stir thoroughly to dissolve, centrifuge and evaporator, place in a vacuum drying oven, and vacuum dry for 1-2 hours to obtain a preservative additive.
[0030] Furthermore, the mass ratio of triphenylphosphine to tannic acid is 1:(18-20), and the mass ratio of hydroquinone monomethyl ether to tannic acid is 1:(280-300).
[0031] Furthermore, the mass ratios of glycidyl methacrylate and glycidyl versatic acid to tannic acid are (1.6-2):1 and 1:(1.4-1.8), respectively.
[0032] Furthermore, the sealing grease comprises, by weight: 16-20 parts of base oil, 10-18 parts of viscosity regulating additives, 8-10 parts of anti-corrosion additives, 1-3 parts of anti-rust additives, 12-16 parts of grease, 10-15 parts of fibers and 20-30 parts of fillers; wherein the base oil is one or more of vegetable oil, polyol ester, polyester, polyether ester and glycerol.
[0033] Furthermore, the fiber is one or more of cotton fiber, polylactic acid fiber, cellulose fiber, chitin fiber and animal fiber.
[0034] Furthermore, the filler is one or more of calcium carbonate, bentonite, talc and kaolin.
[0035] Furthermore, the lubricating grease is one or more of lithium-based lubricating grease, sulfurized lard, lanolin, molybdenum disulfide lubricating grease, and calcium-based lubricating grease.
[0036] Compared with the prior art, the present invention has at least the following beneficial effects:
[0037] 1. The present invention prepares an anti-corrosion additive by mixing n-octane bromide, n-decane bromide and tri-n-butylphosphine for reaction, and then adding the mixture to a mixed solution of mercaptobenzothiazole and potassium hydroxide for further reaction. After adding the anti-corrosion additive to sealing grease, on the one hand, the mercapto group can effectively capture the free radicals generated in the oxidation process of the sealing grease and interrupt the oxidation chain reaction of the grease. On the other hand, the anti-corrosion additive can form a stable complex with metal ions, effectively inhibit the catalytic effect of the metal surface, and reduce the oxidation reaction caused by the metal, thereby achieving the effect of delaying the aging of the grease and improving the corrosion resistance of the grease. In addition, since the anti-corrosion additive rubs against the metal, a tribochemical reaction will occur to generate tribochemical products containing the S element, and these products can form a boundary lubrication film together with the oxide on the metal surface, showing a friction reduction and anti-wear effect, thereby improving the extreme pressure and anti-wear performance of the sealing grease.
[0038] 2. The present invention heats and stirs tannic acid, triphenylphosphine and hydroquinone monomethyl ether, and then adds glycidyl methacrylate and glycidyl versatic acid to react to obtain a viscosity regulating additive. After the viscosity regulating additive is added to the sealing grease, a three-dimensional cross-linked network is formed in the sealing grease, thereby reducing the relative sliding between grease molecules, increasing the intermolecular friction, and enhancing the overall structural strength and viscosity, thereby achieving the effect of improving the cohesiveness and adhesion of the sealing grease, and helping to form a more stable sealing layer.
[0039] 3. The present invention prepares the anti-rust additive by heating and reacting methyl oleate and maleic anhydride, and then mixing with distilled water for hydrolysis reaction. Since the carboxyl end of the anti-rust additive is easily chemically adsorbed with the metal surface to form a dense adsorption film to prevent air and water from contacting the metal to cause rust, the anti-rust additive is added to the sealing grease to effectively improve the anti-rust performance of the sealing grease.
[0040] 4. The sealing grease of the present invention is composed of degradable base oil, fiber and environmentally friendly additives, etc. It is biodegradable, odorless, environmentally friendly and non-toxic, and has no pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.
[0042] Figure 1 This is a process flow chart for preparing the environmentally friendly, biodegradable, and corrosion-resistant sealing grease used in an embodiment of the present invention. DETAILED DESCRIPTION
[0043] The preparation process of an environmentally friendly, degradable, corrosion-resistant sealing grease provided by the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0044] Example 1
[0045] A preparation process of an environmentally friendly biodegradable corrosion-resistant sealing grease, such as Figure 1 As shown, the following steps are included:
[0046] S1: Preparation of anti-rust additives
[0047] Methyl oleate and maleic anhydride are added to a reactor at a molar ratio of 1:1.3, stirred and mixed, heated at 200°C for 8 hours, reacted, and naturally cooled to room temperature to obtain a crude product. Subsequently, the crude product is placed in a vacuum distiller, vacuum distilled to remove impurities, and naturally cooled to room temperature to obtain a precursor. The precursor and distilled water are stirred and mixed at a molar ratio of 1:3, heated at 60°C for 6 hours, hydrolyzed, and then vacuum distilled to remove excess distilled water to obtain an anti-rust additive.
[0048] S2: Preparation of viscosity-adjusting additives
[0049] Tannic acid, ethyl acetate and butyl acetate were added to a reaction tank at a solid-liquid ratio of 15 g: 16 mL: 7 mL, heated at 80 ° C, stirred at a rate of 200 r / min for 30 min, and fully mixed to obtain a mixed solution A, then the heating temperature was kept constant, the stirring rate was adjusted to 100 r / min, triphenylphosphine and hydroquinone monomethyl ether were added to the mixed solution A while stirring, and the stirring was continued for 20 min to obtain a mixed solution B, wherein the mass ratio of triphenylphosphine to tannic acid was 1:18, and the mass ratio of hydroquinone monomethyl ether to tannic acid was 1:280, then, the heating temperature and stirring rate were kept constant, methacrylate glycidyl and Versatic acid glycidyl ester were added to the mixed solution B while stirring, heated for 10 h, and the solvent was removed by reduced pressure distillation to obtain a viscosity regulating additive, wherein the mass ratios of methacrylate glycidyl and Versatic acid glycidyl ester to tannic acid were 1.6:1 and 1:1.4, respectively;
[0050] S3: Preparation of anti-corrosion additives
[0051] n-Bromooctane, n-Bromodecane and tri-n-butylphosphine were stirred and mixed uniformly in a mass ratio of 1:1.2:1, and then heated at 140°C for 10 hours under nitrogen protection for reflux reaction. Impurities were removed by reduced pressure distillation to obtain intermediate A, and then intermediate A was added to methanol in a mass ratio of 1:60, stirred and dissolved to obtain intermediate A solution for standby use, mercaptobenzothiazole and potassium hydroxide were added to methanol in a solid-liquid ratio of 3g:1g:20mL, stirred and dissolved to obtain a ternary mixed solution for standby use, and then intermediate A was ... The intermediate A solution is added to the above ternary mixed solution, and then stirred at a rate of 400r / min for 2h to react to obtain a suspension, wherein the molar ratio of mercaptobenzothiazole to intermediate A is 1:1, and then the suspension is placed in a centrifuge for centrifugal filtration to remove solid impurities, and then the filtrate is rotary evaporated to remove the solvent and water to obtain intermediate B, and finally, the intermediate B is added to anhydrous ethanol, fully stirred to dissolve, and after centrifugal filtration and rotary evaporation, placed in a vacuum drying oven and vacuum dried for 1h to obtain an anticorrosive additive;
[0052] S4: Mix the components to prepare sealing grease
[0053] Add 16 parts of vegetable oil, 1 part of the above-mentioned anti-rust additive, 10 parts of the above-mentioned viscosity regulating additive and 8 parts of the above-mentioned anti-corrosion additive into a kneader and knead for 30 minutes. Then add 12 parts of sulfurized lard into the kneader and continue kneading for 40 minutes. Then add 10 parts of cotton fiber into the kneader and continue kneading for 20 minutes. Then add 20 parts of calcium carbonate into the kneader and continue kneading for 2 hours to obtain sealing grease.
[0054] Example 2
[0055] A preparation process of an environmentally friendly biodegradable corrosion-resistant sealing grease, such as Figure 1 As shown, the following steps are included:
[0056] S1: Preparation of anti-rust additives
[0057] Methyl oleate and maleic anhydride are added to a reactor at a molar ratio of 1:1.5, stirred and mixed, heated at 230°C for 9 hours, reacted, and naturally cooled to room temperature to obtain a crude product. Subsequently, the crude product is placed in a vacuum distiller, vacuum distilled to remove impurities, and naturally cooled to room temperature to obtain a precursor. The precursor and distilled water are stirred and mixed at a molar ratio of 1:4, and then heated at 70°C for 7 hours to perform a hydrolysis reaction. Excess distilled water is removed by vacuum distillation to obtain an anti-rust additive.
[0058] S2: Preparation of viscosity-adjusting additives
[0059] Tannic acid, ethyl acetate and butyl acetate were added to a reaction tank at a solid-liquid ratio of 17.5 g: 18 mL: 8 mL, heated at 85 ° C, stirred at a rate of 250 r / min for 35 min, and fully mixed to obtain a mixed solution A, then the heating temperature was kept constant, the stirring rate was adjusted to 150 r / min, triphenylphosphine and hydroquinone monomethyl ether were added to the mixed solution A while stirring, and the stirring was continued for 25 min to obtain a mixed solution B, wherein the mass ratio of triphenylphosphine to tannic acid was 1:19, and the mass ratio of hydroquinone monomethyl ether to tannic acid was 1:290, then, the heating temperature and stirring rate were kept constant, methacrylate glycidyl and Versatic acid glycidyl ester were added to the mixed solution B while stirring, the reaction was heated for 11 h, and the solvent was removed by reduced pressure distillation to obtain a viscosity regulating additive, wherein the mass ratios of methacrylate glycidyl and Versatic acid glycidyl ester to tannic acid were 1.8:1 and 1:1.6, respectively;
[0060] S3: Preparation of anti-corrosion additives
[0061] n-Bromooctane, n-Bromodecane and tri-n-butylphosphine were stirred and mixed uniformly at a mass ratio of 1:1.3:1.1, and then heated at a temperature of 145°C for 11 hours under nitrogen protection for reflux reaction. Impurities were removed by reduced pressure distillation to obtain intermediate A, and then intermediate A was added to methanol at a mass ratio of 1:65, stirred and dissolved to obtain intermediate A solution, which was set aside, mercaptobenzothiazole and potassium hydroxide were added to methanol at a solid-liquid ratio of 4g:1g:25mL, stirred and dissolved to obtain a ternary mixed solution, which was set aside, and then the intermediate A solution is added to the above ternary mixed solution, and then stirred at a rate of 450r / min for 2.5h to react to obtain a suspension, wherein the molar ratio of mercaptobenzothiazole to intermediate A is 1:1.2, and then the suspension is placed in a centrifuge for centrifugal filtration to remove solid impurities, and then the filtrate is rotary evaporated to remove the solvent and water to obtain intermediate B, and finally, intermediate B is added to anhydrous ethanol, fully stirred to dissolve, and after centrifugal filtration and rotary evaporation, placed in a vacuum drying oven and vacuum dried for 1.5h to obtain an anticorrosive additive;
[0062] S4: Mix the components to prepare sealing grease
[0063] 18 parts of polyol ester, 2 parts of the above-mentioned anti-rust additive, 19 parts of the above-mentioned viscosity regulating additive and 9 parts of the above-mentioned anti-corrosion additive were added to a kneader and kneaded for 35 minutes. Then 14 parts of lanolin were added to the kneader and kneaded for 45 minutes. Then 12 parts of polylactic acid fibers were added to the kneader and kneaded for 25 minutes. Then 25 parts of bentonite were added to the kneader and kneaded for 2.5 hours to obtain sealing grease.
[0064] Example 3
[0065] A preparation process of an environmentally friendly biodegradable corrosion-resistant sealing grease, such as Figure 1 As shown, the following steps are included:
[0066] S1: Preparation of anti-rust additives
[0067] Methyl oleate and maleic anhydride are added to a reactor at a molar ratio of 1:1.8, stirred and mixed, heated at 260°C for 10 hours, reacted, and naturally cooled to room temperature to obtain a crude product. Subsequently, the crude product is placed in a vacuum distiller, vacuum distilled to remove impurities, and naturally cooled to room temperature to obtain a precursor. The precursor and distilled water are stirred and mixed at a molar ratio of 1:5, and then heated at 80°C for 8 hours to perform a hydrolysis reaction. Excess distilled water is removed by vacuum distillation to obtain an anti-rust additive.
[0068] S2: Preparation of viscosity-adjusting additives
[0069] Tannic acid, ethyl acetate and butyl acetate were added to a reaction tank at a solid-liquid ratio of 20 g: 20 mL: 9 mL, heated at 90 ° C, stirred at a rate of 300 r / min for 40 min, and fully mixed to obtain a mixed solution A, then the heating temperature was kept constant, the stirring rate was adjusted to 200 r / min, triphenylphosphine and hydroquinone monomethyl ether were added to the mixed solution A while stirring, and the stirring was continued for 30 min to obtain a mixed solution B, wherein the mass ratio of triphenylphosphine to tannic acid was 1:20, and the mass ratio of hydroquinone monomethyl ether to tannic acid was 1:300, then, the heating temperature and stirring rate were kept constant, methacrylate glycidyl and Versatic acid glycidyl ester were added to the mixed solution B while stirring, the reaction was heated for 12 h, and the solvent was removed by reduced pressure distillation to obtain a viscosity regulating additive, wherein the mass ratios of methacrylate glycidyl and Versatic acid glycidyl ester to tannic acid were 2:1 and 1:1.8, respectively;
[0070] S3: Preparation of anti-corrosion additives
[0071] n-Bromooctane, n-Bromodecane and tri-n-butylphosphine were stirred and mixed uniformly in a mass ratio of 1:1.4:1.2, and then heated at 150°C for 12 hours under nitrogen protection for reflux reaction. Impurities were removed by reduced pressure distillation to obtain intermediate A, and then intermediate A was added to methanol in a mass ratio of 1:70, stirred and dissolved to obtain intermediate A solution for standby use, mercaptobenzothiazole and potassium hydroxide were added to methanol in a solid-liquid ratio of 5g:1g:30mL, stirred and dissolved to obtain a ternary mixed solution for standby use, and then intermediate A was ... The intermediate A solution is added to the above ternary mixed solution, and then stirred at a rate of 500r / min for 3h to react to obtain a suspension, wherein the molar ratio of mercaptobenzothiazole to intermediate A is 1:1.4, and then the suspension is placed in a centrifuge for centrifugal filtration to remove solid impurities, and then the filtrate is rotary evaporated to remove the solvent and water to obtain intermediate B, and finally, the intermediate B is added to anhydrous ethanol, fully stirred to dissolve, and after centrifugal filtration and rotary evaporation, it is placed in a vacuum drying oven and vacuum dried for 2h to obtain an anticorrosive additive;
[0072] S4: Mix the components to prepare sealing grease
[0073] Add 20 parts of polyether ester, 3 parts of the above-mentioned anti-rust additive, 18 parts of the above-mentioned viscosity regulating additive and 10 parts of the above-mentioned anti-corrosion additive into a kneader and knead for 40 minutes. Then add 16 parts of lithium-based grease into the kneader and continue kneading for 50 minutes. Then add 15 parts of cellulose fiber into the kneader and continue kneading for 30 minutes. Then add 30 parts of talc into the kneader and continue kneading for 3 hours to obtain sealing grease.
[0074] The quality test indicators of the sealing grease prepared in Examples 1-3 of the present invention are shown in Table 1 below:
[0075] Table 1: Summary of quality test indicators of sealing grease obtained in Examples 1-3
[0076] Test items Example 1 Example 2 Example 3 Sealing (25℃)MPa 3.5 3.5 3.4 Volatility (80℃, 5h)% 0.12 0.13 0.16 Maximum peeling force (25℃)N 154 152 155 Wear spot diameter (load 800N, 1h) mm 0.85 0.88 0.91 Rust resistance (iron sheet, 100℃, 24h) No rust No rust No rust
[0077] Comparative Example 1
[0078] The difference between this comparative example 1 and embodiment 1 is that the anticorrosive additive in step S4 is removed, and the quality inspection index of the sealing grease obtained is shown in Table 2 below:
[0079] Table 2: Comparison of sealing grease quality test indicators of Example 1 and Comparative Example 1
[0080] Test items Example 1 Comparative Example 1 Volatility (80℃, 5h)% 0.12 0.96 Wear spot diameter (load 800N, 1h) mm 0.85 1.63
[0081] By comparing the sealing grease quality detection indicators of Example 1 and Comparative Example 1, it can be seen that the volatility and wear spot diameter of the sealing grease prepared in Comparative Example 1 without adding the anti-corrosion additive are 0.96% and 1.63 mm, respectively, both of which are greater than the sealing grease prepared in Example 1. It can be seen that the anti-corrosion additive is prepared by first mixing n-octane bromide, n-decane bromide and tri-n-butylphosphine for reaction, and then adding it to a mixed solution of mercaptobenzothiazole and potassium hydroxide for further reaction. After adding it to the sealing grease, on the one hand, the mercapto group can effectively capture the free radicals generated during the oxidation of the sealing grease and interrupt the chain reaction of the grease oxidation. On the other hand, the anti-corrosion additive can form a stable complex with metal ions, effectively inhibit the catalytic effect of the metal surface, and reduce the oxidation reaction caused by the metal, thereby achieving the effect of delaying the aging of the grease and improving the corrosion resistance of the grease. In addition, since the anti-corrosion additive rubs against the metal, a tribochemical reaction will occur to generate tribochemical products containing the S element, and these products can form a boundary lubrication film together with the oxide on the metal surface, showing a friction reduction and anti-wear effect, thereby improving the wear resistance of the sealing grease.
[0082] Comparative Example 2
[0083] The difference between Comparative Example 2 and Example 1 is that the viscosity regulating additive in step S4 is removed, and the quality inspection index of the sealing grease obtained is shown in Table 3 below:
[0084] Table 3: Comparison of sealing grease quality test indicators of Example 1 and Comparative Example 2
[0085] Test items Example 1 Comparative Example 2 Sealing (25℃)MPa 3.5 2.6 Maximum peeling force (25℃)N 154 113
[0086] By comparing the sealing grease quality test indicators of Example 1 and Comparative Example 2, it can be seen that the sealing and maximum peeling force of Comparative Example 2 are 2.6 MPa and 113 N, respectively, which are both less than Example 1. It can be seen that after heating and stirring tannic acid, triphenylphosphine and hydroquinone monomethyl ether, etc., and then adding methacrylate glycidyl ester and Versatic acid glycidyl ester to react to obtain a viscosity regulating additive, after adding the viscosity regulating additive to the sealing grease, it forms a three-dimensional cross-linked network in the sealing grease, thereby reducing the relative sliding between grease molecules, increasing the intermolecular friction, and enhancing the overall structural strength and viscosity, thereby achieving the effect of improving the cohesiveness and adhesion of the sealing grease, and helping to form a more stable sealing layer.
[0087] Comparative Example 3
[0088] The difference between this comparative example 3 and example 1 is that the anti-rust additive in step S4 is removed, and the quality inspection index of the sealing grease obtained is shown in Table 4 below:
[0089] Table 4: Comparison of sealing grease quality test indicators of Example 1 and Comparative Example 3
[0090] Test items Example 1 Comparative Example 3 Rust resistance (iron sheet, 100℃, 24h) No rust Rust
[0091] By comparing the quality inspection indicators of the sealing greases of Example 1 and Example 3, it can be seen that the sealing grease prepared in Example 3 without adding the anti-rust additive cannot prevent moisture and corrosive media from eroding the metal surface, while the sealing grease prepared by adding the anti-rust additive in Example 1 can effectively prevent moisture and corrosive media from eroding the metal surface. It can be seen that the anti-rust additive is prepared by mixing methyl oleate and maleic anhydride, heating them for reaction, and then mixing them with distilled water for hydrolysis reaction. Since the carboxyl end of the anti-rust additive is easily chemically adsorbed with the metal surface to form a dense adsorption film, which prevents air and water from contacting the metal and causing it to rust, the anti-rust additive is added to the sealing grease to effectively improve the anti-rust performance of the sealing grease.
[0092] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease, characterized in that: The steps include: S1: Preparation of anti-rust additives Methyl oleate and maleic anhydride are mixed and heated to react, and then distilled under reduced pressure, and then mixed with distilled water and heated to perform a hydrolysis reaction, and then distilled under reduced pressure again to obtain an anti-rust additive; S2: Preparation of viscosity-adjusting additives Tannic acid, ethyl acetate, butyl acetate, triphenylphosphine and hydroquinone monomethyl ether are stirred and mixed, and glycidyl methacrylate and Versatic acid glycidyl ester are added, and heated to react to obtain a viscosity regulating additive; S3: Preparation of anti-corrosion additives Uniformly mixing n-octane bromide, n-decane bromide and tri-n-butylphosphine to react and prepare intermediate A, dissolving intermediate A in methanol to form intermediate A solution for later use, then dissolving mercaptobenzothiazole and potassium hydroxide in methanol to prepare a ternary mixed solution for later use, and then adding the intermediate A solution to the ternary mixed solution for reaction to obtain an anticorrosive additive; S4: Mix the components to prepare sealing grease Add the base oil, the above-mentioned anti-rust additive, the above-mentioned viscosity regulating additive and the above-mentioned anti-corrosion additive into a kneader, knead for 30-40 minutes, then add the grease into the kneader, continue kneading for 40-50 minutes, then add the fiber into the kneader, continue kneading for 20-30 minutes, then add the filler into the kneader, continue kneading for 2-3 hours to obtain the sealing grease.
2. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: S1 specifically includes the following steps: S1.1: Add methyl oleate and maleic anhydride in a molar ratio of 1:(1.3-1.8) into a reactor, stir and mix well, heat at 200-260°C for 8-10h to react, and cool naturally to room temperature to obtain a crude product; S1.2: placing the crude product in a vacuum distiller, removing impurities by vacuum distillation, and naturally cooling to room temperature to obtain a precursor; S1.3: The above precursor and distilled water are stirred and mixed evenly in a molar ratio of 1:(3-5), and then heated at a temperature of 60-80°C for 6-8h to carry out a hydrolysis reaction, and then the excess distilled water is removed by reduced pressure distillation to obtain an anti-rust additive.
3. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: S2 specifically includes the following steps: S2.1: Mix tannic acid, ethyl acetate and butyl acetate in a solid-liquid ratio of (15-20) g: (16-20) mL: (7-9) mL was added to a reaction tank, heated at 80-90°C, stirred at 200-300 r / min for 30-40 min, and mixed thoroughly to obtain a mixed solution A; S2.2: Keep the heating temperature unchanged, adjust the stirring rate to 100-200 r / min, add triphenylphosphine and hydroquinone monomethyl ether to the mixed solution A while stirring, and continue stirring for 20-30 min to obtain a mixed solution B; S2.3: Keeping the heating temperature and stirring rate unchanged, add glycidyl methacrylate and glycidyl versatic acid to the mixed solution B while stirring, heat the reaction for 10-12 hours, and remove the solvent by vacuum distillation to obtain a viscosity regulating additive.
4. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: S3 specifically includes the following steps: S3.1: n-octane bromide, n-decane bromide and tri-n-butylphosphine are stirred and mixed uniformly in a mass ratio of 1:(1.2-1.4):(1-1.2), and then heated at 140-150° C. for 10-12 h under nitrogen protection to reflux reaction, and impurities are removed by reduced pressure distillation to obtain intermediate A; S3.2: Add the intermediate A to methanol at a mass ratio of 1:(60-70), stir thoroughly to dissolve, and obtain an intermediate A solution; S3.3: Add mercaptobenzothiazole and potassium hydroxide to methanol at a solid-liquid ratio of (3-5) g: 1 g: (20-30) mL, stir thoroughly to dissolve, and obtain a ternary mixed solution; S3.4: adding the intermediate A solution to the ternary mixed solution, and then stirring at a rate of 400-500 r / min for 2-3 hours to react to obtain a suspension, wherein the molar ratio of mercaptobenzothiazole to intermediate A is 1:(1-1.4); S3.5: Place the above suspension in a centrifuge and perform centrifugal filtration to remove solid impurities, then perform rotary evaporation on the filtrate to remove the solvent and water to obtain intermediate B; S3.6: Add the intermediate B mentioned above to anhydrous ethanol, stir thoroughly to dissolve, centrifuge and evaporator, place in a vacuum drying oven, and vacuum dry for 1-2 hours to obtain a preservative additive.
5. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 3, characterized in that: The mass ratio of triphenylphosphine to tannic acid is 1:(18-20), and the mass ratio of hydroquinone monomethyl ether to tannic acid is 1:(280-300).
6. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 3, characterized in that: The mass ratios of glycidyl methacrylate and glycidyl versatic acid to tannic acid are (1.6-2):1 and 1:(1.4-1.8), respectively.
7. The process for preparing an environmentally friendly biodegradable corrosion-resistant sealing grease according to claim 1, characterized in that: The sealing grease comprises, by weight: 16-20 parts of base oil, 10-18 parts of viscosity regulating additives, 8-10 parts of anti-corrosion additives, 1-3 parts of anti-rust additives, 12-16 parts of grease, 10-15 parts of fiber and 20-30 parts of filler; wherein the base oil is one or more of vegetable oil, polyol ester, polyester, polyether ester and glycerol.
8. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: The fiber is one or more of cotton fiber, polylactic acid fiber, cellulose fiber, chitin fiber and animal fiber.
9. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: The filler is one or more of calcium carbonate, bentonite, talc and kaolin.
10. The process for preparing an environmentally friendly, degradable, corrosion-resistant sealing grease according to claim 1, characterized in that: The lubricating grease is one or more of lithium-based lubricating grease, sulfurized lard, lanolin, molybdenum disulfide lubricating grease, and calcium-based lubricating grease.
Citation Information
Patent Citations
Degradable type shield tail sealing grease of shield excavation machine
CN102757839A
Wide-temperature-range urea-based shield tail sealing grease and preparation method thereof
CN111303976A
Epoxy grease-based unsaturated ester light-cured resin, preparation method therefor and use thereof
WO2019020010A1
Cited By
Water-based acrylic resin-based rotor antirust agent and processing method thereof
CN120623867A
Aqueous acrylic resin-based rotor antirust agent and its processing method
CN120623867B