Faucet and preparation method thereof
By injecting filler into the inner liner of the faucet for high-pressure casting, the problems of low efficiency and poor consistency of the existing faucet preparation process are solved, and direct contact between the stainless steel faucet and water is achieved, simplifying the structure and reducing costs.
Patent Information
- Application Number
- CN202410826776.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing metal faucet preparation process is low efficiency, the product appearance is irregular, the consistency is poor, the inner wall is rough and easy to cause sand holes, and zinc alloy and aluminum alloy faucets cannot directly contact with the running water, so plastic pipes need to be added, resulting in an increase in costs.
Use an inner liner with a cavity, inject the inner liner filler for high-pressure casting, and after removing the filler, the faucet is obtained. The inner liner material is stainless steel, the filler is resin sand, etc., which improves the compressive strength, avoids vacuuming operations, and simplifies the valve core. structure.
It improves the compressive strength and consistency of the faucet, simplifies the preparation process, reduces costs, and avoids the use of plastic pipes. The inner wall of the product is smooth and uniform in thickness.
Smart Images

Figure BDA0004910728080000071 
Figure BDA0004910728080000081 
Figure BDA0004910728080000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of faucets, and in particular to a faucet and a preparation method thereof. Background Art
[0002] Metal faucets currently occupy a certain proportion in the market. They are mainly produced by traditional low-pressure casting technology. Specifically, after the sand core is formed, the cast metal alloy is injected into the mold cavity under a relatively low pressure to form the faucet. Then the sand core is removed to form a space for water to flow inside the faucet. The traditional sand core is mainly made of resin material, and its compressive strength is 60-80kg / cm 2 , it is impossible to use the high-pressure casting process, and the preparation process has the following main disadvantages: first, low efficiency; second, the product appearance is irregular, the consistency is poor, and the product surface is rough, which is easy to have sand holes; the inner wall of the product is rough, and the residue of the sand core cannot be completely cleaned, leaving residues on the inner wall, causing the residues to fall off during the electroplating process, causing pollution to the electroplating tank. In addition, zinc alloy and aluminum alloy metal faucets can hardly come into direct contact with running water, and often need to add plastic pipes to the inner wall of the faucet to provide a water flow channel. Due to the limited plasticity of plastic pipes, the appearance of the faucet is extremely restricted, and the valve core structure is complex, which will increase costs.
[0003] The applicant provided a faucet and its preparation method and a mold for producing faucets in CN115464116A, using an inner shell with a hollow cavity to replace the filling core in the prior art, and the inner shell is injected with filling oil to support the inner shell. After forming, there is no need for core pulling, and the filling oil can be directly discharged to obtain a faucet with a smooth cavity. This method has high production efficiency, saves materials, and the wall thickness of the faucet is uniform. However, this preparation method has high technical requirements and cannot be industrialized. Therefore, the applicant has made improvements on this basis to reduce the technical difficulty of the faucet in process production. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a preparation process for a faucet with a simple preparation process and low difficulty. The faucet inner shell prepared by the improved preparation method is made of stainless steel material and can be in direct contact with water. The inner shell is smooth, the product appearance is regular, and the consistency is high.
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a faucet in a first aspect, comprising:
[0006] (1) preparing an inner container having a cavity;
[0007] (2) injecting a liner filler into the cavity of the liner and forming the filler in the cavity;
[0008] (3) placing the inner liner filled with the inner liner filler in a mold, performing high-pressure casting, and removing the inner liner filler in the cavity after cooling and forming, thereby obtaining a faucet;
[0009] The inner liner filler is one or more of resin, silica gel, foam material, resin sand, steel balls, cement, sawdust mixture, flour, wax, ice, and dry ice; the raw material for preparing the inner liner is at least one of stainless steel, titanium alloy, copper, and aluminum.
[0010] As an improvement of the above solution, the compressive strength of the inner liner with the inner liner filler is 200-600 kg / cm 2 .
[0011] As an improvement of the above solution, the inner liner is prepared by stamping, drawing, expansion, welding and CNC machining processes, and the thickness of the inner liner is 0.1-1 mm.
[0012] As an improvement of the above scheme, when the wall thickness of the stainless steel is 0.5 mm, the compressive strength is 70-90 kg / cm 2 ;
[0013] The chemical composition of the stainless steel is calculated by mass percentage as follows: C≤0.08%, Cr=16.00-20.00%, Ni=8.00-15.00%, Si≤1.00%, Mn≤2.00%, and P≤0.045%.
[0014] As an improvement of the above solution, the inner liner filler is pressed and formed under pressure after entering the inner liner, the pressure is 0.2-0.6Mpa, and the particle size range of the inner liner filler is 150-900μm.
[0015] As an improvement of the above solution, the inner tank filler is resin sand, and the strength of the resin sand after pressing is 8-80kg / cm 2 ;
[0016] The volume of the inner liner filler in the cavity after compression molding accounts for 95-98%.
[0017] As an improvement of the above solution, the proportion of resin in the resin sand is 0.4-0.9wt%; the fluidity of the resin sand is 25-30°;
[0018] In the resin sand, particles of 250-350 μm account for 5-7%, particles of 400-450 μm account for 69-73%, and particles of 550-650 μm account for 20-24%;
[0019] The melting point of the resin sand is 105-115°C.
[0020] As an improvement of the above solution, the inner liner filling in the cavity is removed by high-frequency vibration, or the inner liner filling in the cavity is removed by mechanical processing.
[0021] As an improvement of the above solution, the injection pressure during high-pressure casting is 20-100 MPa, the injection time is 0.01 s-0.5 s, and the molding time is 0.01 s-0.5 s.
[0022] The second aspect of the present invention further provides a faucet, which is prepared by the above-mentioned faucet preparation method.
[0023] The implementation of the present invention has the following beneficial effects:
[0024] In the present invention, an inner liner with a cavity is first prepared, and then an inner liner filler is injected into the cavity of the inner liner, and the cavity is filled and formed, and then placed in a mold for casting. After cooling and forming, the inner liner filler in the cavity is removed to obtain a faucet, thereby avoiding the operation of vacuuming, reducing the difficulty of industrial production, and simplifying and improving the preparation process. In addition, by injecting the inner liner filler into the inner liner, the compressive strength of the inner liner is effectively improved, so that the faucet can be prepared using a high-pressure casting process, and the setting of the inner liner allows the faucet to directly contact water, avoiding the setting of a conventional plastic pipe, simplifying the valve core structure of the faucet, and reducing costs. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described in detail with specific embodiments below.
[0026] In order to solve the above problems, the first aspect of the present invention provides a method for preparing a faucet, comprising:
[0027] (1) preparing an inner container having a cavity;
[0028] (2) injecting a liner filler into the cavity of the liner and forming the filler in the cavity;
[0029] (3) placing the inner tank filled with the inner tank filler in a mold, performing high-pressure casting, and removing the inner tank filler in the cavity after cooling and forming, thereby obtaining a faucet.
[0030] The resin sand core used in the preparation process of traditional faucets is easily dispersed by high pressure, because it will cause irregular deformation of the inner wall and appearance, resulting in poor consistency of the product. In the present invention, the vacuum operation is avoided, and the inner liner filler can be directly added to the inner liner, which reduces the difficulty of the preparation process and improves the preparation efficiency. In addition, by preparing an inner liner with a cavity and injecting the inner liner filler into the inner liner, the pressure resistance of the inner liner can be increased, making it suitable for high-pressure casting process, and the inner liner can be in direct contact with water, avoiding the setting of plastic pipes in the inner wall of the faucet, which helps to simplify the structure of the faucet valve core, thereby reducing production costs.
[0031] Preferably, the compressive strength of the inner liner with the inner liner filler is 200-600 kg / cm 2 .
[0032] Preferably, in step (1), the raw material for preparing the inner liner is at least one of stainless steel, titanium alloy, copper and aluminum.
[0033] Furthermore, when the wall thickness of the stainless steel is 0.5 mm, the compressive strength is 70 to 90 kg / cm 2 . It should be noted that the compressive strength of the stainless steel here is obtained by testing a stainless steel standard block with a size of 11.8mm (height) * 22mm (width) * 70mm (length) * 0.5mm (wall thickness) as a sample. The chemical composition of the stainless steel is calculated by mass percentage as follows: C≤0.08%, Cr=16.00~20.00%, Ni=8.00~15.00%, Si≤1.00%, Mn≤2.00%, P≤0.045%. While ensuring the strength of the inner liner, it can also ensure that it can be in direct contact with water to avoid the precipitation of metal elements during long-term use and affect its use. Among them, the C content, Si content, Mn content, and Ni content will significantly affect the strength and corrosion resistance of the resulting inner liner, and thus affect its safety of use and service life. More preferably, the stainless steel complies with European and / or American standards regarding stainless steel materials for drinking water, and the stainless steel includes but is not limited to models such as 304, 304L, 306, 316, and 316L.
[0034] Preferably, the inner liner is prepared by stamping, stretching, expansion, welding and CNC machining processes, and the thickness of the inner liner is 0.1-1 mm. If the thickness of the inner liner is too thin, its strength will be reduced, and deformation will occur during the casting process, making the wall thickness of the resulting faucet uneven. If the thickness of the inner liner is too thick, it will increase the difficulty of removing the inner liner filler in the inner liner, and it will increase the difficulty of preparing the inner liner, reducing production efficiency. More preferably, the thickness of the inner liner is 0.3-1 mm.
[0035] The separate inner liner of the present invention is only improved in terms of raw materials and thickness, and its own strength is still unable to withstand high pressure, that is, the faucet cannot be prepared using a high-pressure casting process. Therefore, an inner liner filler is added to the inner liner, and the inner liner filler is pressed and formed under pressure after entering the inner liner, and the filling and forming are realized in the cavity, and the inner liner is combined with the inner liner, which can effectively improve the compressive strength of the inner liner and greatly improve its compressive resistance.
[0036] Preferably, in step (2), the liner filler is in powder form, and the particle size of the liner filler is in the range of 150 to 900 μm. After the liner filler enters the liner, it is pressed under pressure, and the pressure during pressing is 0.2 to 0.6 MPa, so as to ensure that there is no loose structure on the surface of the resin sand after pressing. If the particle size of the liner filler is too large, the pores between the liner fillers will be too large and cannot be formed, or too much pressure will be required for pressing, and too much pressure may cause deformation of the liner. However, if the particle size of the liner filler is too small, there will be a problem of poor powder fluidity, which will lead to problems such as uneven thickness after pressing and inability to completely fill the cavity. In addition, the smoothness of the inner wall of the liner and the uniformity of thickness can be maintained by controlling the pressing pressure.
[0037] Furthermore, the liner filler is one or more of resin, silica gel, foam material, resin sand, steel ball, cement, sawdust mixture, flour, wax, ice, and dry ice. The liner filler may also be other conventional powders, including but not limited to gypsum powder, rice flour, starch, iron powder, copper powder, aluminum powder, and any combination thereof. Specifically, one or more of resin sand, resin, silica gel, foam material, steel ball, cement, sawdust, flour, and wax may be uniformly mixed, and then pressed and formed under the action of pressure. The obtained mixture is used as the liner filler, and the compressive strength of the liner during high-pressure casting is reasonably adjusted to meet the casting conditions within a larger pressure range, and the fluidity, temperature resistance stability, etc. of the liner filler may also be adjusted. When ice or dry ice is selected as the liner filler, the high-pressure casting time is short, which can ensure that the ice or dry ice will not melt, thereby providing sufficient compressive strength. In special cases, thermal insulation materials may also be provided.
[0038] In some preferred and specific embodiments, the inner tank filler is resin sand, and the strength of the resin sand after pressing is 8-80 kg / cm 2 , and the volume of the inner liner filler in the cavity after compression molding accounts for 95-98%. The inner liner filler with compressive strength combined with the inner liner of a specific thickness can increase the compressive strength of the inner liner by more than 3 times compared to a single inner liner or pressed resin sand, and can withstand higher pressures. In addition, it can be completely dispersed and removed by high-frequency vibration treatment at a later stage, and the treatment method is simple.
[0039] Furthermore, the resin content in the resin sand is 0.4-0.9wt%, the fluidity of the resin sand is 25-30°, and the strength and viscosity of the resin sand as a liner filler can be taken into account at the same time. The particles of 250-350μm in the resin sand account for 5-7%, the particles of 400-450μm account for 69-73%, and the particles of 550-650μm account for 20-24%. More preferably, the particles of 300μm in the resin sand account for 5-7%, the particles of 425μm account for 69-73%, and the particles of 600μm account for 20-24%. The melting point of the resin sand is 105-115°C, and the curing time of the resin sand is about 70s, which is conducive to forming a dense liner filler during pressing, and further makes the compressive strength of the resin sand liner filler reach 10kg / cm 2 The above can further improve the compressive strength of the inner liner to 200-600kg / cm 2 , which is suitable for casting under higher pressure conditions. The content of resin in resin sand, or the refinement of resin sand particles, is conducive to increasing the compressive strength of the stainless steel liner after the resin sand is filled, but it will make the sand cleaning more difficult. If conventional resin sand materials are used as liner fillers, they are filled in the stainless steel liner, which cannot significantly improve the compressive strength of the stainless steel liner, and thus the high-pressure casting process cannot be used to prepare the faucet, and the inner wall of the prepared faucet will be rough and the product consistency will be poor.
[0040] In other preferred and specific embodiments, the liner filler is resin sand and silica gel, and the weight ratio of the resin sand and silica gel is (1-2): 1, and the particle size range of the silica gel is 150-500 μm, and the Shore hardness is 50-90. By evenly mixing the resin sand and silica gel of specific accessories as the liner filler, the two can act synergistically to improve the fluidity of the liner filler, and form a dense and stable filling body under pressure, which can then be combined with the stainless steel liner to effectively improve the compressive strength of the stainless steel liner, and make the inner wall of the stainless steel liner obtained by high-pressure casting smooth, and the product consistency is high. More preferably, the particle size range of the silica gel is 150-250 μm, and the Shore hardness is 70-90, which has good bonding performance with the resin sand in the present invention, and the formed liner filler has suitable fluidity, further improving the compressive strength of the stainless steel liner, and is easy to remove later.
[0041] Preferably, the liner filler in the cavity is removed by high-frequency vibration. The removal method is simple and efficient, which further improves the preparation efficiency. Moreover, the liner filler in the cavity can be completely removed, effectively avoiding the contamination of the electroplating liquid in the later electroplating cylinder. At the same time, it can also ensure that the structure of the faucet will not be affected, and the bend of the faucet will not be deformed or damaged. Of course, the liner filler in the cavity can also be removed by mechanical processing, which can be listed as manual tool removal, mechanical milling, drilling, grinding, etc., which are not specifically limited in the present invention.
[0042] Preferably, in step (3), high pressure casting is used for casting, the injection pressure is 20 to 100 MPa, the injection time is 0.01 s to 0.5 s, and the molding time is 0.01 s to 0.5 s; more preferably, the injection pressure is 20 to 55 MPa.
[0043] The second aspect of the present invention further provides a faucet, which is prepared by the above-mentioned preparation method.
[0044] The present invention will be further described below with specific embodiments:
[0045] Example 1
[0046] This embodiment provides a faucet, which is prepared by the following method:
[0047] (1) The inner liner with a cavity is prepared by stamping, stretching, expansion, CNC machining, and welding processes;
[0048] The raw material for preparing the liner is stainless steel, and the chemical composition is as follows by mass percentage: C≤0.08%, Cr=18.00-20.00%, Ni=8.00-10.00%, Si≤1.00%, Mn≤2.00%, P≤0.045%, the thickness of the liner is 0.5mm, and the size is 11.18mm*22.16mm*70mm;
[0049] (2) injecting resin sand into the cavity of the liner and filling and molding the cavity;
[0050] The relevant parameters of the resin sand are as follows: the proportion of resin is 0.6wt%, the melting point is 110°C, the hardening time is 70s, the fluidity (angle of repose) is 27.17°, and the particles of 300μm in the resin sand account for 5-7%, the particles of 425μm account for 69-73%, and the particles of 600μm account for 20-24%.
[0051] After the resin sand enters the inner tank, it is pressed and formed under pressure, the pressure is 0.4MPa, and the volume of the resin sand in the cavity after pressing and forming accounts for 97%;
[0052] (3) The inner shell filled with resin sand is placed in a mold and high-pressure casting is performed. The injection pressure is 25 MPa, the injection time is 0.1 s, and the molding time is 0.3 s. After cooling and molding, the resin in the cavity is removed by high-frequency vibration to obtain a faucet.
[0053] Example 2
[0054] This embodiment provides a faucet, which is basically the same as the embodiment 1, except that:
[0055] The thickness of the liner is 0.3mm.
[0056] Example 3
[0057] This embodiment provides a faucet, which is basically the same as the embodiment 1, except that:
[0058] The thickness of the liner is 1mm;
[0059] High pressure casting was performed with an injection pressure of 50 MPa.
[0060] Example 4
[0061] This embodiment provides a faucet, which is basically the same as the embodiment 1, except that:
[0062] Resin sand and silica gel are injected into the cavity of the inner tank, and the cavity is filled and formed, wherein the mass ratio of resin sand to silica gel is 2:1, the particle size range of silica gel is 150-250μm, the Shore A hardness is 70-90, and the viscosity.
[0063] Performance Testing
[0064] 1. By means of compression test, referring to GB / T 7314-2017, the compressive strength of the resin sand liner filler, the stainless steel liner and the liner filled with the liner filler after compression molding in the embodiment was tested. The dimensions of the three samples to be tested were 11.18mm*22.16mm*70mm, and the wall thickness of the liner was 0.5mm. The test results are shown in Table 1 below.
[0065] Table 1 Test results of strength in Examples 1-4
[0066]
[0067]
[0068] From the above results, it can be seen that by filling the inner liner of the stainless steel material with resin sand and adjusting and optimizing the thickness of the inner liner, its compressive resistance can be effectively improved, so that it can better meet the high-pressure casting process, and the effect is better when the wall thickness of the stainless steel inner liner is 0.5mm~1.0mm. In addition, resin sand and other powders such as silica gel are selected as the inner liner filler to further improve the compressive strength of the stainless steel inner liner.
[0069] 2. The wall thickness of the faucet obtained in the embodiment and the roughness of the inner wall of the inner tank were tested. The testing method was to divide the faucet obtained in the embodiment into 4 equal parts along the length direction, and set each equal part as a test point, and obtain 4 test points respectively. The wall thickness and the roughness of the inner wall of the cavity were tested at these 4 test points, and the average wall thickness and average roughness of these 4 points were calculated and recorded. The test results are shown in Table 2.
[0070] Table 2 Test results of wall thickness and roughness of inner wall of liner of Examples 1-4
[0071]
[0072]
[0073] From the above results, it can be seen that the present invention avoids the vacuum operation by providing an inner tank and filling the inner tank with specific resin sand, simplifies the preparation method, and when the inner tank wall thickness of the obtained faucet is 0.5-1.0 mm, the inner wall is smooth, the thickness is uniform, and it has a high degree of consistency.
[0074] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A method for preparing a faucet, characterized in that: include: (1) preparing an inner container having a cavity; (2) injecting a liner filler into the cavity of the liner and forming the filler in the cavity; (3) placing the inner liner filled with the inner liner filler in a mold, performing high-pressure casting, and removing the inner liner filler in the cavity after cooling and forming, thereby obtaining a faucet; The inner liner filler is one or more of resin, silica gel, foam material, resin sand, steel balls, cement, sawdust mixture, flour, wax, ice, and dry ice; the raw material for preparing the inner liner is at least one of stainless steel, titanium alloy, copper, and aluminum.
2. The method for preparing a faucet according to claim 1, characterized in that: The compressive strength of the inner liner with the inner liner filler is 200-600 kg / cm 2 .
3. The method for preparing a faucet according to claim 1, characterized in that: The inner liner is prepared by stamping, drawing, expansion, welding and numerical control processing technology, and the thickness of the inner liner is 0.1-1 mm.
4. The method for preparing a faucet according to claim 1, characterized in that: When the wall thickness of the stainless steel is 0.5 mm, the compressive strength is 70-90 kg / cm 2 ; The chemical composition of the stainless steel is calculated by mass percentage as follows: C≤0.08%, Cr=16.00-20.00%, Ni=8.00-15.00%, Si≤1.00%, Mn≤2.00%, and P≤0.045%.
5. The method for preparing a faucet according to claim 1, characterized in that: After the inner liner filler enters the inner liner, it is pressed and formed under pressure, the pressure is 0.2-0.6Mpa, and the particle size range of the inner liner filler is 150-900μm.
6. The method for preparing a faucet according to claim 1 or 5, characterized in that: The inner tank filler is resin sand, and the strength of the resin sand after pressing is 8-80kg / cm 2 ; The volume of the inner liner filler in the cavity after compression molding accounts for 95-98%.
7. The method for preparing a faucet according to claim 6, characterized in that: The resin content in the resin sand is 0.4-0.9wt%; the fluidity of the resin sand is 25-30°; In the resin sand, particles of 250-350 μm account for 5-7%, particles of 400-450 μm account for 69-73%, and particles of 550-650 μm account for 20-24%; The melting point of the resin sand is 105-115°C.
8. The method for preparing a faucet according to claim 1, characterized in that: The inner liner filling in the cavity is removed by high-frequency vibration, or the inner liner filling in the cavity is removed by mechanical processing.
9. The method for preparing a faucet according to claim 1, characterized in that: The injection pressure during high pressure casting is 20-100 MPa, the injection time is 0.01s-0.5s, and the molding time is 0.01s-0.5s.
10. A faucet, characterized in that: The faucet is prepared by the preparation method of the faucet as described in any one of claims 1 to 9.
Citation Information
Cited By
Faucet and manufacturing method thereof
US12722201B2
Faucet and manufacturing method therefor
WO2026002284A1