Solid-liquid mixed propellant and preparation method thereof
By introducing a combustion regulator system of tetramethyl ammonium octahydrotriborate and auxiliary combustion regulator into the solid-liquid mixed propellant, the problems of long ignition delay period and low combustion speed are solved, and the combustion speed is increased and the ignition delay is achieved. The period is shortened, the scope of application has been expanded, and a solid foundation is provided for the development of solid-liquid hybrid rocket engines.
Patent Information
- Application Number
- CN202411148423.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The long ignition delay period and low combustion speed of solid-liquid mixed propellant limit its application range.
Using a combustion regulator system including tetramethyloctahydrotriborate and auxiliary combustion regulator, combined with specific adhesives and solid fuel formulations, solid-liquid mixed propellants are prepared through premix and wall-mounted casting processes to optimize liquid oxidants and solid propellant ratio.
It significantly shortens the ignition delay period of solid-liquid mixed propellant, improves the combustion speed, expands the application range, and lays the foundation for the development of solid-liquid mixed rocket engines.
Smart Images

Figure CN118878385A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solid-liquid mixed propellants, and in particular to a solid-liquid mixed propellant and a preparation method thereof. Background Art
[0002] The solid-liquid hybrid rocket engine is an important development direction of rocket propulsion system, and has gradually developed into an important competitor of solid and liquid engines, with broad application prospects. The solid-liquid hybrid rocket engine is a propulsion system between liquid rocket engines and solid rocket engines. The liquid oxidizer system is similar to the oxidizer system of liquid rocket engines, and the fuel column, engine casing and nozzle are similar to solid rocket engines. Compared with liquid engines, the number of pipes, pumps and other moving parts of solid-liquid hybrid engines is only half of that of liquid engines, so the reliability is relatively high; compared with solid engines, the engine thrust adjustment, multiple starts and shutdowns can be realized; therefore, this propulsion system has the advantages of high safety and reliability, excellent performance, and multiple shutdowns and starts.
[0003] Solid-liquid hybrid propellants are composed of solid fuel and liquid oxidizer, but the low burning rate and long ignition delay of solid fuel grains restrict the application of solid-liquid hybrid propellants. At present, the burning rate is improved by adding new adhesive polydicyclopentadiene (DCPD), adding metal hydrides, and adding a small amount of KClO4; there are studies on hybrid propellants, solid fuel formulas have been developed, and solid-liquid engine tests with diameters of 100mm, 120mm, 300mm and 500mm have been carried out. The average burning rate is 0.96-1.10mm / s, and the ignition delay is 126ms; but there are no related research reports on solid-liquid hybrid propellants that can shorten the ignition delay. Summary of the invention
[0004] In view of the above problems, a first object of the present invention is to provide a solid-liquid mixed propellant having the advantage of a small ignition delay period.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned solid-liquid mixed propellant.
[0006] The first technical solution adopted by the present invention is: a solid-liquid mixed propellant, including a solid propellant and a liquid oxidizer, wherein the solid propellant includes the following components by mass percentage:
[0007] Adhesive system: 15% to 20%;
[0008] Solid fuel: 60%~70%;
[0009] Auxiliary metal fuel: 10%~20%;
[0010] Combustion regulator: 1.5% to 3%;
[0011] Performance regulator: 0.2% to 1%;
[0012] Wherein, the combustion regulator comprises tetramethylammonium octahydrogen triborate and an auxiliary combustion regulator, and the mass ratio of the tetramethylammonium octahydrogen triborate to the auxiliary combustion regulator is 4:1.
[0013] Preferably, the liquid oxidant is fuming nitric acid, and the mass ratio of the liquid oxidant to the solid propellant is 3:1.
[0014] Preferably, the auxiliary combustion regulator is one or more of ferric oxide, catocene, copper chromite and n-octylferrocene.
[0015] Preferably, the tetramethylammonium octahydrogen triborate is prepared by the following method:
[0016] Using ethylene glycol dimethyl ether as solvent, diborane and potassium borohydride react under the conditions of 0.3-0.6MPa and 30-50°C to prepare tetramethylammonium octahydrotriborate.
[0017] Preferably, the adhesive system includes an adhesive, a curing agent and a plasticizer, and the mass ratio of the adhesive, the curing agent and the plasticizer is 13.10-16.15:0.95-1.05:3; the adhesive is terminal hydroxyl polybutadiene; the curing agent is one or more of toluene diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate; the plasticizer is one or more of diisooctyl sebacate and acetyl tributyl citrate.
[0018] Preferably, the solid fuel is octahydro-s-tetrazine-(1,2-a)-s-tetrazine.
[0019] Preferably, the octahydro-tetrazine-(1,2-a)-tetrazine is prepared by the following method:
[0020] Octahydro-s-tetrazine-(1,2-a)-s-tetrazine can be prepared by reacting hydrazine and formaldehyde at 30°C to 50°C.
[0021] Preferably, the auxiliary metal fuel is one or more of aluminum powder and magnesium powder.
[0022] Preferably, the performance regulator is one or more of tris(-2-methylaziridine-1)phosphine oxide, triphenylbismuth, ferric acetylacetonate, triethanolamine boron trifluoride, and methylene 4426-S.
[0023] The second technical solution adopted by the present invention is: a method for preparing the solid-liquid mixed propellant as described in the first technical solution, comprising the following steps:
[0024] S1: In a dry environment, weigh each component in proportion, add a combustion regulator, a performance regulator, and a plasticizer to the adhesive, and add an auxiliary metal fuel for premixing to obtain a premixed slurry;
[0025] S2: adding the premixed slurry into a mixer, and adding solid fuel in batches for mixing, adding a curing agent after all components are fully mixed and continuing to mix evenly to obtain a slurry;
[0026] S3: pouring the slurry into the engine by sticking to the wall to obtain a solid propellant, and storing the liquid oxidizer separately in an oxidizer tank to obtain a solid-liquid mixed propellant.
[0027] Beneficial effects of the above technical solution:
[0028] (1) Compared with similar domestic solid-liquid mixed propellants, the solid-liquid mixed propellant disclosed in the present invention has the advantage of a short ignition delay period.
[0029] (2) The present invention provides a solid-liquid hybrid propellant with a short ignition delay period for a solid-liquid hybrid engine, which uses a new type of high-efficiency combustion regulator to increase the burning rate of the solid-liquid hybrid propellant and significantly shorten the ignition delay time of the solid-liquid hybrid propellant.
[0030] (3) The solid-liquid mixed propellant provided by the present invention introduces a new type of high-efficiency combustion regulator to improve the combustion performance of the solid-liquid mixed propellant, shorten the ignition delay time, and further improve the burning rate of the solid-liquid mixed propellant without changing the ratio of the liquid oxidizer and the solid propellant; thereby solving the problems of long ignition delay period and low burning rate of the solid-liquid mixed propellant, expanding the application scope of the solid-liquid mixed propellant, laying a solid foundation for the development of the power device of the solid-liquid mixed rocket engine, and significantly enhancing my country's national defense strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a process flow chart of a method for preparing a solid-liquid mixed propellant. DETAILED DESCRIPTION
[0032] The present invention is further described below through specific embodiments. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the principle of the present invention, and these should also be regarded as belonging to the protection scope of the present invention.
[0033] The contents not described in detail in the specification of the present invention belong to the common knowledge of the professionals in this field.
[0034] The present invention discloses a solid-liquid mixed propellant, comprising a solid propellant and a liquid oxidant, wherein the solid propellant comprises the following components by mass percentage:
[0035] Adhesive system: 15% to 20%;
[0036] Solid fuel: 60%~70%;
[0037] Auxiliary metal fuel: 10%~20%;
[0038] Combustion regulator: 1.5% to 3%;
[0039] Performance regulator: 0.2% to 1%;
[0040] The mass ratio of the liquid oxidizer to the solid propellant is 3:1.
[0041] Among them, the new high-efficiency combustion regulator is mainly composed of tetramethylammonium octahydrogen triborate, and the auxiliary combustion regulator is one or more of ferric oxide (Fe2O3), catocene (GFP), copper chromite (CC) and n-octylferrocene (T27); that is, the combustion regulator includes tetramethylammonium octahydrogen triborate and the auxiliary combustion regulator, and the mass ratio of the tetramethylammonium octahydrogen triborate and the auxiliary combustion regulator is 4:1.
[0042] The tetramethylammonium octahydrogen triborate is prepared by the following method:
[0043] 900-950 ml of ethylene glycol dimethyl ether is used as a solvent, and diborane and potassium borohydride are reacted for 12-13 hours under the conditions of 0.3-0.6 MPa and 30-50° C. to prepare tetramethylammonium octahydrotriborate; the mass ratio of the diborane to the potassium borohydride is 23:44.
[0044] The adhesive system comprises an adhesive, a curing agent and a plasticizer, wherein the mass ratio of the adhesive, the curing agent and the plasticizer in the adhesive system is 13.10-16.15:0.95-1.05:3; the adhesive is hydroxy-terminated polybutadiene (HTPB); the curing agent is one or more of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI) and hexamethylene diisocyanate (HDI); and the plasticizer is one or more of diisooctyl sebacate (DOS) and acetyl tributyl citrate (ATBC).
[0045] The solid fuel is octahydro-tetrazine-(1,2-a)-tetrazine, and the octahydro-tetrazine-(1,2-a)-tetrazine is prepared by the following method:
[0046] The octahydro-s-tetrazine-(1,2-a)-s-tetrazine can be prepared by reacting hydrazine and formaldehyde at 30°C to 50°C; the mass ratio of hydrazine to formaldehyde is 4:5.
[0047] The auxiliary metal fuel is one or more of aluminum powder and magnesium powder.
[0048] The performance regulator is one or more of tris(-2-methylaziridine-1)phosphine oxide (MAPO), triphenylbismuth (TPB), ferric acetylacetonate (FeAA), triethanolamine boron trifluoride (TEA), and methylene 4426-S (Hs).
[0049] The liquid oxidant is fuming nitric acid (FNA).
[0050] like Figure 1 As shown, the solid-liquid hybrid propellant is prepared by the following steps:
[0051] S1: In a dry environment, weigh each component in proportion, add a combustion regulator, a performance regulator, and a plasticizer to the adhesive, and add an auxiliary metal fuel for premixing to obtain a premixed slurry;
[0052] S2: adding the premixed slurry into a mixer, and adding solid fuel octahydro-tetrazine-(1,2-a)-tetrazine in batches for mixing, adding a curing agent after all components are fully mixed and continuing to mix evenly to obtain a slurry;
[0053] S3: The slurry is poured into the engine by sticking to the wall (vacuum pouring into the engine and placing in a dry environment at about 60°C for 7 days to cure) to obtain a solid propellant; and the liquid oxidant is stored separately in an oxidant tank to obtain a solid-liquid mixed propellant; when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when in contact with the solid propellant.
[0054] The prepared solid-liquid hybrid propellant was characterized as follows:
[0055] 1) Density: measured in accordance with standard QJ 917A-1997 "Determination of density of composite solid propellants, linings and insulation materials";
[0056] 2) Ignition delay time is measured in accordance with the standards GJB96A-2020 "Standard test engine types and dimensions" and GJB97A-2020 "Technical requirements and data processing for standard test engines";
[0057] 3) The maximum tensile strength and maximum elongation shall be measured in accordance with the standard GJB770B-2022 "Explosive Powder Test Method".
[0058] Example 1
[0059] Weigh each material according to the formula in Table 1 (calculated by mass percentage):
[0060] Table 1 Composition formula of solid-liquid mixed propellant
[0061]
[0062] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0063] The properties of the prepared solid-liquid mixed propellant were measured, and the results are shown in Table 2.
[0064] Table 2 Properties of solid-liquid mixed propellants
[0065]
[0066] Example 2
[0067] Weigh each material according to the formula in Table 3 (calculated by mass percentage):
[0068] Table 3 Composition formula of solid-liquid mixed propellant
[0069]
[0070]
[0071] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0072] The properties of the prepared solid-liquid mixed propellant were measured, and the results are shown in Table 4.
[0073] Table 4 Solid-liquid mixed propellant properties
[0074]
[0075] Example 3
[0076] Weigh each material according to the formula in Table 5 (calculated by mass percentage):
[0077] Table 5 Composition formula of solid-liquid mixed propellant
[0078]
[0079] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0080] The properties of the prepared solid-liquid mixed propellant were measured, and the results are shown in Table 6.
[0081] Table 6 Solid-liquid mixed propellant properties
[0082]
[0083] Example 4
[0084] Weigh each material according to the formula in Table 7 (calculated by mass percentage):
[0085] Table 7 Solid-liquid mixed propellant composition formula
[0086]
[0087] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0088] The prepared solid-liquid mixed propellant was tested for various properties, and the test results are shown in Table 8.
[0089] Table 8 Solid-liquid mixed propellant properties
[0090]
[0091] Example 5
[0092] Weigh each material according to the formula in Table 9 (calculated by mass percentage):
[0093] Table 9 Composition formula of solid-liquid mixed propellant
[0094]
[0095]
[0096] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0097] The properties of the prepared solid-liquid mixed propellant were measured, and the measurement results are shown in Table 10.
[0098] Table 10 Solid-liquid mixed propellant properties
[0099]
[0100] Example 6
[0101] Weigh each material according to the formula in Table 11 (calculated by mass percentage):
[0102] Table 11 Solid-liquid mixed propellant composition formula
[0103]
[0104] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0105] The properties of the prepared solid-liquid mixed propellant were measured, and the results are shown in Table 12.
[0106] Table 12 Properties of solid-liquid mixed propellants
[0107]
[0108] Example 7
[0109] Weigh each material according to the formula in Table 13 (calculated by mass percentage):
[0110] Table 13 Solid-liquid mixed propellant composition formula
[0111]
[0112] The combustion regulator, performance regulator and plasticizer weighed above are added to the adhesive, and the auxiliary metal fuel is added for premixing to obtain a premixed slurry; the premixed slurry is added to the mixer, and the solid fuel octahydro-tetrazine-(1,2-a)-tetrazine is added in batches for mixing, and after each component is fully mixed, a curing agent is added and continued to be mixed evenly to obtain a slurry; the slurry is vacuum poured into the engine, and placed in a dry environment at about 60°C for curing for 7 days to obtain a solid propellant. The liquid oxidant is stored separately in the oxidant tank, and when the engine needs to work, the liquid oxidant is sprayed on the surface of the solid propellant, and the liquid oxidant can burn when it contacts the solid propellant.
[0113] The properties of the prepared solid-liquid mixed propellant were measured, and the measurement results are shown in Table 14.
[0114] Table 14 Properties of solid-liquid mixed propellants
[0115]
[0116] Comparative Example 1
[0117] The following table shows the formula composition and performance of the closest solid-liquid mixed propellant for comparison.
[0118] (1) Solid-liquid mixed propellant composition
[0119]
[0120] (2) Performance of solid-liquid hybrid propellants
[0121]
[0122] It can be seen from the data in Example 1 and Comparative Example 1 that the density, maximum tensile strength and maximum elongation of the solid-liquid mixed propellant prepared in Comparative Example 1 and Example 1 are equivalent, but the ignition delay period of the solid-liquid mixed propellant disclosed in the present invention is significantly shortened: the ignition delay period of Comparative Example 1 is 686ms, while the ignition delay period of the solid-liquid mixed propellant of the present invention does not exceed 50ms.
[0123] The present invention is described in detail above in combination with specific implementation methods and exemplary examples. The above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments; the above description cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, the technical solution of the present invention and its implementation methods may be subjected to a variety of equivalent substitutions, modifications or improvements, all of which fall within the scope of the present invention; the protection scope of the present invention shall be subject to the attached claims.
Claims
1. A solid-liquid hybrid propellant, comprising a solid propellant and a liquid oxidizer, characterized in that: The solid propellant comprises the following components by mass percentage: Adhesive system: 15% to 20%; Solid fuel: 60%~70%; Auxiliary metal fuel: 10% to 20%; Combustion regulator: 1.5% to 3%; Performance regulator: 0.2% to 1%; Wherein, the combustion regulator comprises tetramethylammonium octahydrogen triborate and an auxiliary combustion regulator, and the mass ratio of the tetramethylammonium octahydrogen triborate to the auxiliary combustion regulator is 4:
1.
2. The solid-liquid hybrid propellant according to claim 1, characterized in that: The liquid oxidant is fuming nitric acid, and the mass ratio of the liquid oxidant to the solid propellant is 3:
1.
3. The solid-liquid hybrid propellant according to claim 1, characterized in that: The auxiliary combustion regulator is one or more of ferric oxide, catocene, copper chromite and n-octylferrocene.
4. The solid-liquid hybrid propellant according to claim 1, characterized in that: The tetramethylammonium octahydrogen triborate is prepared by the following method: Using ethylene glycol dimethyl ether as solvent, diborane and potassium borohydride react under the conditions of 0.3-0.6MPa and 30-50°C to prepare tetramethylammonium octahydrogentriborate.
5. The solid-liquid hybrid propellant according to claim 1, characterized in that: The adhesive system includes an adhesive, a curing agent and a plasticizer, wherein the mass ratio of the adhesive, the curing agent and the plasticizer is 13.10-16.15:0.95-1.05:3; the adhesive is terminal hydroxyl polybutadiene; the curing agent is one or more of toluene diisocyanate, isophorone diisocyanate and hexamethylene diisocyanate; and the plasticizer is one or more of diisooctyl sebacate and acetyl tributyl citrate.
6. The solid-liquid hybrid propellant according to claim 1, characterized in that: The solid fuel is octahydro-tetrazine-(1,2-a)-tetrazine.
7. The solid-liquid hybrid propellant according to claim 6, characterized in that: The octahydro-tetrazine-(1,2-a)-tetrazine is prepared by the following method: Octahydro-s-tetrazine-(1,2-a)-s-tetrazine can be prepared by reacting hydrazine and formaldehyde at 30°C to 50°C.
8. The solid-liquid hybrid propellant according to claim 1, characterized in that: The auxiliary metal fuel is one or more of aluminum powder and magnesium powder.
9. The solid-liquid hybrid propellant according to claim 1, characterized in that: The performance regulator is one or more of tris(-2-methylaziridine-1)phosphine oxide, triphenyl bismuth, ferric acetylacetonate, triethanolamine boron trifluoride, and methylene 4426-S.
10. A method for preparing the solid-liquid hybrid propellant according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1: In a dry environment, weigh each component in proportion, add a combustion regulator, a performance regulator, and a plasticizer to the adhesive, and add an auxiliary metal fuel for premixing to obtain a premixed slurry; S2: adding the premixed slurry into a mixer, and adding solid fuel in batches for mixing, adding a curing agent after all components are fully mixed and continuing to mix evenly to obtain a slurry; S3: pouring the slurry into the engine by sticking to the wall to obtain a solid propellant, and storing the liquid oxidizer separately in an oxidizer tank to obtain a solid-liquid mixed propellant.
Citation Information
Patent Citations
Boron-containing fuel-rich propellant
CN109574773A
High-burning-rate propellant for platform combustion and preparation method thereof
CN112898106A
Ammonia borane solid propellant
CN119504323A
Method for preparing ammonium octahydro-triborate via double decomposition
CN85100255A
Cold solid propellant; pyrotechnic loading; methods of obtaining same
EP1985599A2