Perfluoropolyether-based polyurethane urea elastic sealing material as well as preparation method and application thereof
By developing a method for preparing perfluoropolyether-based polyurethane urea elastomers, the problem of insufficient strength, toughness, and shape memory properties of perfluoroether rubber in extremely low-temperature environments has been solved, enabling the application of high-strength and tough sealing materials in the range of -80℃ to 30℃.
Patent Information
- Application Number
- CN202410913009.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Existing perfluoroelastomer rubbers cannot meet the requirements for high strength and toughness and shape memory performance in response to heat and light stimulation at extremely low temperatures, and are particularly ineffective in sealing and shock absorption in specific working environments such as aerospace.
The preparation method of perfluoropolyether-based polyurethane urea elastomer adopts a method that introduces polysiloxane and perfluoropolyether as soft segments and urethane and urea as hard segments through nucleophilic addition reaction and crosslinking polymerization reaction to form dynamic reversible hydrogen bonds, thereby improving the strength and toughness of the material. Pentaerythritol is added to adjust the degree of crosslinking.
The prepared perfluoropolyether-based polyurethane urea elastomer maintains good tensile strength and toughness in the range of -80℃ to 30℃, and has self-healing and heat-stimulated responsive shape memory properties, making it suitable for sealing and shock absorption in extreme low-temperature environments.
Smart Images

Figure CN118878780A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane urea elastomers, and specifically relates to a perfluoropolyether-based polyurethane urea elastic sealing material and a preparation method and application thereof. Background Art
[0002] In addition to being used as sealing materials, low-temperature elastomers can also be used as tires, cable sheaths, cushions, etc., and play an irreplaceable role in extreme environments such as the Antarctic and the Moon. In specific working environments such as aerospace, such as the outlet joints of liquid hydrogen and liquid oxygen devices, the temperature may drop to a low temperature range (below -150°C), which is far below the elastic temperature range of polymer materials. Therefore, the development of polymer materials that can exhibit good elasticity at extremely low temperatures of -80°C or even below -100°C is one of the urgent problems to be solved in the field of polar or aerospace science and technology.
[0003] In the extremely demanding field of sealing and shock absorption, perfluoroether elastomers, as special fluorinated polymers, are highly favored due to their excellent oil resistance, medium resistance, high and low temperature resistance. Although commercial perfluoroether rubbers have been widely used in high-end fields such as aerospace, commercial perfluoroether rubbers cannot meet the use requirements, such as ultra-low temperature working environment, high strength and toughness, repairability, thermal and optical stimulus response shape memory performance, etc. Therefore, the development of new perfluoropolyether (PFPE)-based polymer materials is the most effective way to solve the above limitations. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a perfluoropolyether-based polyurethane urea elastic sealing material and a preparation method and application thereof. The perfluoropolyether-based polyurethane urea elastomer obtained by the preparation method provided by the present invention has excellent tensile strength and toughness, a wide operating temperature range, and can maintain good tensile strength in an environment of -80°C to 30°C.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a perfluoropolyether-based polyurethane urea elastomer, comprising the following steps:
[0007] The bis(1-hydroxymethyl)-terminated perfluoropolyether, isocyanate and dibutyltin dilaurate are mixed and subjected to a first nucleophilic addition reaction to obtain a perfluoropolyether-based polyurethane elastomer;
[0008] The bis(1-hydroxymethyl) terminated perfluoropolyether has a structure shown in Formula 1:
[0009]
[0010] The perfluoropolyether-based polyurethane elastomer, bis(3-aminopropyl)-terminated polydimethylsiloxane and an organic solvent are mixed, a second nucleophilic addition reaction is carried out, pentaerythritol is added, a cross-linking polymerization reaction occurs, and a perfluoropolyether-based polyurethane urea elastomer is obtained;
[0011] The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to isocyanate is 1:1.5-2.5;
[0012] The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1-5:1-5;
[0013] The molar ratio of the pentaerythritol to the bis(1-hydroxymethyl)-terminated perfluoropolyether is 0-2:1-5.
[0014] Preferably, the isocyanate includes 4,4-diisocyanate dicyclohexylmethane, isophorone diisocyanate, hexamethylene diisocyanate or toluene diisocyanate.
[0015] Preferably, the ratio of the volume of the dibutyltin dilaurate to the molar amount of the bis(1-hydroxymethyl)-terminated perfluoropolyether is 20-60 μL:1-5 mmol.
[0016] Preferably, the molecular weight of the bis(1-hydroxymethyl)-terminated perfluoropolyether is 2 to 4 kDa;
[0017] The molecular weight of the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1 to 5 kDa.
[0018] Preferably, the temperature of the first nucleophilic addition reaction is 70-90° C. and the time is 2-4 h.
[0019] Preferably, the temperature of the second nucleophilic addition reaction is 20-30° C. and the time is 20-30 h.
[0020] Preferably, the cross-linking polymerization reaction is carried out at a temperature of 20 to 30° C. and for a time of 4 to 8 hours.
[0021] Preferably, the organic solvent includes one or more of N,N-dimethylacetamide, chlorobenzene, fluorobenzene, tetrahydrofuran and 1,4-dioxane.
[0022] The present invention also provides a perfluoropolyether-based polyurethane urea elastomer prepared by the preparation method described in the above technical solution.
[0023] The present invention also provides application of the perfluoropolyether-based polyurethane urea elastomer described in the above technical solution in sealing materials.
[0024] The invention provides a method for preparing a perfluoropolyether-based polyurethane urea elastomer, comprising the following steps: mixing a bis(1-hydroxymethyl)-terminated perfluoropolyether, isocyanate and dibutyltin dilaurate, and performing a first nucleophilic addition reaction to obtain a perfluoropolyether-based polyurethane elastomer; mixing the perfluoropolyether-based polyurethane elastomer, a bis(3-aminopropyl)-terminated polydimethylsiloxane and an organic solvent, and performing a second nucleophilic addition reaction; adding pentaerythritol, and performing a crosslinking polymerization reaction to obtain a perfluoropolyether-based polyurethane urea elastomer; the molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the isocyanate is 1:1.5-2.5; the molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1-5:1-5; and the molar ratio of the pentaerythritol to the bis(1-hydroxymethyl)-terminated perfluoropolyether is 0-2:1-5. The present invention uses low-temperature flexible polysiloxane and perfluoropolyether as soft segments, and urethane bonds and urea bonds formed by the reaction as hard segments, and prepares perfluoropolyether (PFPE)-based polyurethane urea elastomer through a flexible chain "two-in-one" strategy. The introduction of two low-temperature flexible chains can effectively reduce the glass transition temperature of polyurethane urea, and the introduction of urethane bonds and urea bonds allows a large number of dynamic reversible hydrogen bonds to exist in the molecular chain, thereby improving the strength and toughness of the material; the presence of pentaerythritol further increases the hydrogen bonding effect between polyurethane urea segments, increases the sacrificial bond energy, and from the perspective of energy dissipation mechanism, the gradient hydrogen bond array formed by urethane bonds and urea bonds can significantly improve the mechanical properties of PFPE-type polyurethane urea elastomer; by controlling the amount of pentaerythritol, the crosslinking degree of PFPE-based polyurethane urea elastomer is changed, and elastomers with different oil resistance are obtained. The method provided by the present invention is simple to operate, and the obtained PFPE-based polyurethane urea elastomer can maintain good sealing performance in a low-temperature fuel environment.
[0025] The present invention also provides a PFPE-based polyurethane urea elastomer prepared by the preparation method described in the above technical scheme, with a room temperature tensile strength of ≥1.0MPa, a room temperature elongation at break of ≥100%, a Shore hardness D of ≥55, an operating temperature of -80°C to 30°C, a tensile strength of not less than 14MPa at -80°C, and a toughness of not less than 18MJ / m 3 It has excellent tensile strength and toughness, as well as low-temperature resistance, and its swelling rate in kerosene is ≤15%. It can be used as an extreme service material in the field of low-temperature fuel sealing and shock absorption.
[0026] At the same time, PFPE-based polyurethane urea elastomers can have properties such as self-repairing, processability and recycling, and thermal stimulus responsive shape memory through the synergistic effect of dynamic covalent bonds and hydrogen bonds. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0028] Figure 1 The tensile strength and elongation at break curves of the PFPE-based polyurethane urea elastomers prepared in Examples 1 to 5;
[0029] Figure 2 Typical room temperature tensile curves of PFPE-based polyurethane urea elastomers prepared in Examples 1 to 5;
[0030] Figure 3 This is a tensile curve of the PFPE-based polyurethane urea elastomer prepared in Example 4 at -80°C;
[0031] Figure 4 It is the swelling ratio of the PFPE-based polyurethane urea elastomer prepared in Examples 1 to 5 in kerosene. DETAILED DESCRIPTION
[0032] The present invention provides a method for preparing a perfluoropolyether-based polyurethane urea elastomer, comprising the following steps:
[0033] The bis(1-hydroxymethyl)-terminated perfluoropolyether, isocyanate and dibutyltin dilaurate are mixed and subjected to a first nucleophilic addition reaction to obtain a perfluoropolyether-based polyurethane elastomer;
[0034] The perfluoropolyether-based polyurethane elastomer, bis(3-aminopropyl)-terminated polydimethylsiloxane and an organic solvent are mixed, a second nucleophilic addition reaction is carried out, pentaerythritol is added, a cross-linking polymerization reaction occurs, and a perfluoropolyether-based polyurethane urea elastomer is obtained;
[0035] The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to isocyanate is 1:1.5-2.5;
[0036] The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1-5:1-5;
[0037] The molar ratio of the pentaerythritol to the bis(1-hydroxymethyl)-terminated perfluoropolyether is 0-2:1-5.
[0038] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0039] In the present invention, before the operation, the bis(1-hydroxymethyl)-terminated perfluoropolyether and the bis(3-aminopropyl)-terminated polydimethylsiloxane are preferably dehumidified, preferably at 90-95° C. for 1-2 hours in vacuum. By dehumidification, the moisture in the prepolymer is removed to avoid side reactions.
[0040] The invention mixes bis(1-hydroxymethyl)-terminated perfluoropolyether, isocyanate and dibutyltin dilaurate, and generates a first nucleophilic addition reaction to obtain a perfluoropolyether-based polyurethane elastomer.
[0041] In the present invention, the molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to isocyanate is preferably 1:1.5 to 2.5, more preferably 1:1.6 to 2.0, and further preferably 1:1.7 to 1.9.
[0042] In the present invention, the isocyanate preferably includes 4,4-diisocyanate dicyclohexylmethane, isophorone diisocyanate, hexamethylene diisocyanate or toluene diisocyanate, more preferably 4,4-diisocyanate dicyclohexylmethane or toluene diisocyanate, and further preferably 4,4-diisocyanate dicyclohexylmethane.
[0043] In the present invention, the molecular weight of the bis(1-hydroxymethyl)-terminated perfluoropolyether is preferably 2 to 4 kDa, more preferably 2.5 to 3 kDa. The bis(1-hydroxymethyl)-terminated perfluoropolyether in the present invention has a structure shown in Formula 1:
[0044]
[0045] In the present invention, the volume ratio of the dibutyltin dilaurate to the molar amount of the bis(1-hydroxymethyl)-terminated perfluoropolyether is preferably 20-60 μL:1-5 mmol, more preferably 24-55 μL:2-4 mmol, and further preferably 45 μL:4 mmol.
[0046] The present invention has no special requirements for the mixing, and conventional means in the art can be used. In a specific embodiment of the present invention, after the bis(1-hydroxymethyl)-terminated perfluoropolyether and isocyanate are mixed, dibutyltin dilaurate is added dropwise.
[0047] In the present invention, the temperature of the first nucleophilic addition reaction is preferably 70 to 90° C., more preferably 75 to 85° C., and the time is preferably 2 to 4 hours, more preferably 2.5 to 3.5 hours.
[0048] In the present invention, the first nucleophilic addition reaction preferably further comprises cooling, and the cooling temperature is preferably 20-30° C., more preferably 22-28° C. During the first nucleophilic addition reaction, isocyanate and hydroxyl react to form urethane bonds to obtain a perfluoropolyether-based polyurethane elastomer.
[0049] After obtaining the perfluoropolyether-based polyurethane elastomer, the present invention mixes the perfluoropolyether-based polyurethane elastomer, bis(3-aminopropyl)-terminated polydimethylsiloxane and an organic solvent to cause a second nucleophilic addition reaction, and then adds pentaerythritol to cause a cross-linking polymerization reaction to obtain a perfluoropolyether-based polyurethane urea elastomer.
[0050] In the present invention, the molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1 to 5: 1 to 5, preferably 2 to 4: 2 to 4. In a specific embodiment of the present invention, the molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1: 1 or 2: 1.
[0051] In the present invention, the molecular weight of the bis(3-aminopropyl)-terminated polydimethylsiloxane is preferably 1 to 5 kDa, more preferably 1.5 to 4 kDa, and further preferably 2 to 3 kDa. The bis(3-aminopropyl)-terminated polydimethylsiloxane in the present invention has a structure shown in Formula 2:
[0052]
[0053] In the present invention, the organic solvent preferably includes one or more of N,N-dimethylacetamide, chlorobenzene, fluorobenzene, tetrahydrofuran and 1,4-dioxane, more preferably one or more of N,N-dimethylacetamide, chlorobenzene, fluorobenzene and tetrahydrofuran, and further preferably N,N-dimethylacetamide, fluorobenzene or tetrahydrofuran. In the present invention, the ratio of the volume of the organic solvent to the molar amount of the bis(1-hydroxymethyl)-terminated perfluoropolyether is preferably 20-50mL:1-5mmol, more preferably 30-40mL:2-4mmol. In a specific embodiment of the present invention, the ratio of the volume of the organic solvent to the molar amount of the bis(1-hydroxymethyl)-terminated perfluoropolyether is 30mL:2mmol or 40mL:4mmol or 30mL:4mmol.
[0054] The present invention has no special requirements for the mixing, and conventional means in the art can be used. In a specific embodiment of the present invention, after the perfluoropolyether-based polyurethane elastomer and the organic solvent are mixed, bis(3-aminopropyl)-terminated polydimethylsiloxane is added.
[0055] In the present invention, the temperature of the second nucleophilic addition reaction is preferably 20 to 30° C., more preferably 22 to 28° C., and the time is preferably 20 to 30 hours, more preferably 24 to 26 hours. During the second nucleophilic addition reaction, the amino group in the bis(3-aminopropyl)-terminated polydimethylsiloxane reacts with the isocyanate to form a urea bond.
[0056] In the present invention, the molar ratio of pentaerythritol to bis(1-hydroxymethyl)-terminated perfluoropolyether is 0-2:1-5, preferably 0.2-1:2-4. In a specific embodiment of the present invention, the molar ratio of pentaerythritol to bis(1-hydroxymethyl)-terminated perfluoropolyether is 0:2 or 0.1:2. In the present invention, the pentaerythritol is preferably used in the form of a dissolving solution; the dissolving solution is preferably obtained by dissolving pentaerythritol in an organic solvent; the type of the organic solvent is the same as above. The concentration of the dissolving solution is preferably 0.01-0.2 mmol / mL.
[0057] In the present invention, the temperature of the cross-linking polymerization reaction is preferably 20 to 30° C., more preferably 22 to 28° C., and the time is preferably 4 to 8 hours, more preferably 5 to 6 hours.
[0058] In the present invention, the preparation of the perfluoropolyether-based polyurethane urea elastomer complies with the following reaction formula 3:
[0059]
[0060] After the cross-linking polymerization reaction is completed, the obtained perfluoropolyether-based polyurethane urea elastomer is a solution. Those skilled in the art can dry the perfluoropolyether-based polyurethane urea elastomer solution according to actual needs to obtain a solid perfluoropolyether-based polyurethane urea elastomer. In the present invention, the drying temperature is preferably 40 to 80° C., and the drying time is preferably 24 to 26 hours. In a specific embodiment of the present invention, a polytetrafluoroethylene mold is used for drying in a blast drying oven.
[0061] The present invention also provides a perfluoropolyether-based polyurethane urea elastomer prepared by the preparation method described in the above technical solution.
[0062] The present invention is based on the concept of polymer molecular structure design, takes the energy dissipation mechanism of dynamic reversible bonds as the criterion, and utilizes the "flexible chain two-in-one" strategy to accurately prepare a perfluoropolyether (PFPE)-based polyurethane urea elastomer with polysiloxane and perfluoropolyether as soft segments and urethane bonds and urea bonds as hard segments. The soft segment can effectively reduce the glass transition temperature of the polyurethane urea, while the hard segment enables the presence of a large number of dynamically reversible hydrogen bonds in the molecular chain, which can improve the strength and toughness of the material.
[0063] The present invention also provides the use of the perfluoropolyether-based polyurethane urea elastomer described in the above technical solution in sealing materials.
[0064] In the present invention, the application environment temperature of the sealing material is preferably -80°C to 30°C.
[0065] The present invention has no particular limitation on the specific manner of the application, and any manner familiar to those skilled in the art may be used.
[0066] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.
[0067] Example 1
[0068] The bis(1-hydroxymethyl)-terminated perfluoropolyether and bis(3-aminopropyl)-terminated polydimethylsiloxane were placed in a 95°C oven for vacuum dehumidification for 1 hour. 4.0 g (2.0 mmol) of bis(1-hydroxymethyl)-terminated perfluoropolyether and 1.05 g (4.0 mmol) of 4,4-diisocyanate dicyclohexylmethane were placed in a 100 mL three-necked flask, 3 drops of dibutyltin dilaurate were added thereto, the three-necked flask was placed in an oil bath preheated to 70°C, reacted for 4 hours, cooled to room temperature, 30 mL of N,N-dimethylacetamide and 5.0 g (2.0 mmol) of bis(3-aminopropyl)-terminated polydimethylsiloxane were added to the three-necked flask, and stirred at room temperature for 24 hours to obtain a PFPE-based polyurethane urea elastomer solution.
[0069] The PFPE-based polyurethane urea elastomer solution was placed in a polytetrafluoroethylene mold, and the mold was placed in a forced air drying oven and dried at 80° C. for 24 hours to obtain a PFPE-based polyurethane urea elastomer.
[0070] Example 2
[0071] The bis(1-hydroxymethyl)-terminated perfluoropolyether and bis(3-aminopropyl)-terminated polydimethylsiloxane were placed in a 95°C oven for vacuum dehumidification for 1 hour. 8.0 g (4.0 mmol) of bis(1-hydroxymethyl)-terminated perfluoropolyether and 1.68 g (6.4 mmol) of 4,4-diisocyanate dicyclohexylmethane were placed in a 100 mL three-necked flask, 3 drops of dibutyltin dilaurate were added thereto, the three-necked flask was placed in an oil bath preheated to 70°C, reacted for 4 hours, cooled to room temperature, 40 mL of tetrahydrofuran and 5.0 g (2.0 mmol) of bis(3-aminopropyl)-terminated polydimethylsiloxane were added to the three-necked flask, stirred at room temperature for 24 hours, 10 mL of N,N-dimethylacetamide, including 27.23 mg (0.2 mmol) of pentaerythritol, reacted at room temperature for 4 hours, and a PFPE-based polyurethane urea elastomer solution was obtained.
[0072] The PFPE-based polyurethane urea elastomer solution was placed in a polytetrafluoroethylene mold, and the mold was placed in a forced air drying oven and dried at 40° C. for 24 hours to obtain a PFPE-based polyurethane urea elastomer.
[0073] Example 3
[0074] The bis(1-hydroxymethyl)-terminated perfluoropolyether and bis(3-aminopropyl)-terminated polydimethylsiloxane were placed in a 95°C oven for vacuum dehumidification for 1 hour. 8.0 g (4.0 mmol) of bis(1-hydroxymethyl)-terminated perfluoropolyether and 1.78 g (6.8 mmol) of 4,4-diisocyanate dicyclohexylmethane were placed in a 100 mL three-necked flask, 3 drops of dibutyltin dilaurate were added thereto, the three-necked flask was placed in an oil bath preheated to 70°C, reacted for 4 hours, cooled to room temperature, 40 mL of fluorobenzene and 5.0 g (2.0 mmol) of bis(3-aminopropyl)-terminated polydimethylsiloxane were added to the three-necked flask, stirred at room temperature for 24 hours, 10 mL of N,N-dimethylacetamide, including 54.46 mg (0.4 mmol) of pentaerythritol, were added, and reacted at room temperature for 4 hours to obtain a PFPE-based polyurethane urea elastomer solution.
[0075] The PFPE-based polyurethane urea elastomer solution was placed in a polytetrafluoroethylene mold, and the mold was placed in a forced air drying oven and dried at 50° C. for 24 hours to obtain a PFPE-based polyurethane urea elastomer.
[0076] Example 4
[0077] The bis(1-hydroxymethyl)-terminated perfluoropolyether and the bis(3-aminopropyl)-terminated polydimethylsiloxane were placed in an oven at 95° C. for vacuum dehumidification for 1 h. 8.0 g (4.0 mmol) of bis(1-hydroxymethyl)-terminated perfluoropolyether and 1.994 g (7.6 mmol) of 4,4-diisocyanate dicyclohexylmethane were placed in a 100 mL three-necked flask, 3 drops of dibutyltin dilaurate were added thereto, the three-necked flask was placed in an oil bath preheated to 70°C, the reaction was continued for 4 hours, the mixture was cooled to room temperature, 30 mL of N,N-dimethylacetamide and 5.0 g (2.0 mmol) of bis(3-aminopropyl)-terminated polydimethylsiloxane were added to the three-necked flask, the mixture was stirred at room temperature for 24 hours, 10 mL of N,N-dimethylacetamide, including 108.92 mg (0.8 mmol) of pentaerythritol, the mixture was reacted at room temperature for 4 hours, and a PFPE-based polyurethane urea elastomer solution was obtained.
[0078] The PFPE-based polyurethane urea elastomer solution was placed in a polytetrafluoroethylene mold, and the mold was placed in a forced air drying oven and dried at 80° C. for 24 hours to obtain a PFPE-based polyurethane urea elastomer.
[0079] Example 5
[0080] The bis(1-hydroxymethyl)-terminated perfluoropolyether and the bis(3-aminopropyl)-terminated polydimethylsiloxane were placed in an oven at 95° C. for vacuum dehumidification for 1 h. 8.0 g (4.0 mmol) of bis(1-hydroxymethyl)-terminated perfluoropolyether and 2.2 g (8.4 mmol) of 4,4-diisocyanate dicyclohexylmethane were placed in a 100 mL three-necked flask, 3 drops of dibutyltin dilaurate were added thereto, the three-necked flask was placed in an oil bath preheated to 70°C, the reaction was continued for 4 hours, the mixture was cooled to room temperature, 30 mL of N,N-dimethylacetamide and 5.0 g (2.0 mmol) of bis(3-aminopropyl)-terminated polydimethylsiloxane were added to the three-necked flask, the mixture was stirred at room temperature for 24 hours, 10 mL of N,N-dimethylacetamide, including 163.38 mg (1.2 mmol) of pentaerythritol, the mixture was reacted at room temperature for 4 hours, and a PFPE-based polyurethane urea elastomer solution was obtained.
[0081] The PFPE-based polyurethane urea elastomer solution was placed in a polytetrafluoroethylene mold, and the mold was placed in a forced air drying oven and dried at 80° C. for 24 hours to obtain a PFPE-based polyurethane urea elastomer.
[0082] According to GB / T 528-2009, the tensile stress-strain properties of vulcanized rubber or thermoplastic rubber are measured, the room temperature tensile strength and elongation at break are measured on a universal tensile testing machine, the sample shape is dumbbell-shaped, the effective test size is 2.0 mm in width, 0.5 mm in thickness, 150 mm in length, and the tensile speed is 10 mm / min. The swelling rate is measured according to GB / T 1690-2010, the liquid resistance test method of vulcanized rubber or thermoplastic rubber, and the Shore hardness (D) is measured using a hardness tester according to GB / T 2411-2008, plastics and hard rubber. The relevant test data of the PFPE-based polyurethane urea prepared in Examples 1 to 5 are plotted in Table 1.
[0083] Table 1 Test results of PFPE-based polyurethane urea elastomers prepared in Examples 1 to 5
[0084] Example 1 Example 2 Example 3 Example 4 Example 5 Room temperature (25°C) tensile strength / MPa 1.6 1.8 2.8 4.8 5.1 Elongation at break at room temperature (25°C) / % 114.6 248.6 525.7 512.7 224.5 -80℃ tensile strength / MPa / / / 14.7 / -80℃ breaking elongation / % / / / 191.2 / <![CDATA[-80 °C toughness / MJ / m 3 > / / / 18 / Swelling rate in kerosene / % 14.3 13.1 10.7 8.3 6.7 Shore Hardness D 55 57 59 61 67
[0085] Figure 1 The tensile strength and elongation at break curves of the PFPE-based polyurethane urea elastomers prepared in Examples 1 to 5 are shown in FIG. Figure 2 It is a typical room temperature tensile curve diagram of the PFPE-based polyurethane urea elastomer prepared in Examples 1 to 5, wherein Samples 1 to 5 correspond to Examples 1 to 5 respectively. Figure 3 This is a tensile curve of the PFPE-based polyurethane urea elastomer prepared in Example 4 at -80°C. Figures 1 to 3It can be seen that the PFPE-based polyurethane urea elastomer obtained by the present invention has a tensile strength of ≥1.0 MPa, an elongation at break of ≥100%, a kerosene swelling ratio of ≤15%, a Shore hardness of ≥55, and an operating temperature of -80°C to 30°C. It can exhibit excellent tensile strength and toughness in a -80 environment. This indicates that the PFPE-based polyurethane urea elastomer obtained by the present invention has good sealing performance in a low-temperature fuel environment.
[0086] Figure 4 is the swelling ratio of the PFPE-based polyurethane urea elastomer prepared in Examples 1 to 5 in kerosene, wherein Samples 1 to 5 correspond to Examples 1 to 5 in sequence. Figure 4 It can be seen that the swelling rate of the PFPE-based polyurethane urea elastomer prepared in Examples 1 to 5 in kerosene is less than 15%, indicating that the elastomer has good kerosene resistance; and as the degree of crosslinking increases, the swelling rate decreases and the oil resistance of the elastomer increases.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a perfluoropolyether-based polyurethane urea elastomer, It is characterized in that The following steps are involved: The bis(1-hydroxymethyl)-terminated perfluoropolyether, isocyanate and dibutyltin dilaurate are mixed and subjected to a first nucleophilic addition reaction to obtain a perfluoropolyether-based polyurethane elastomer; The bis(1-hydroxymethyl) terminated perfluoropolyether has a structure shown in Formula 1: The perfluoropolyether-based polyurethane elastomer, bis(3-aminopropyl)-terminated polydimethylsiloxane and an organic solvent are mixed, a second nucleophilic addition reaction is carried out, pentaerythritol is added, a cross-linking polymerization reaction occurs, and a perfluoropolyether-based polyurethane urea elastomer is obtained; The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to isocyanate is 1:1.5-2.5; The molar ratio of the bis(1-hydroxymethyl)-terminated perfluoropolyether to the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1-5:1-5; The molar ratio of the pentaerythritol to the bis(1-hydroxymethyl)-terminated perfluoropolyether is 0-2:1-5.
2. The preparation method according to claim 1, It is characterized in that The isocyanate includes 4,4-diisocyanate dicyclohexylmethane, isophorone diisocyanate, hexamethylene diisocyanate or toluene diisocyanate.
3. The preparation method according to claim 1 or 2, It is characterized in that The ratio of the volume of the dibutyltin dilaurate to the molar amount of the bis(1-hydroxymethyl)-terminated perfluoropolyether is 20-60 μL:1-5 mmol.
4. The preparation method according to claim 1, It is characterized in that The molecular weight of the bis(1-hydroxymethyl) terminated perfluoropolyether is 2 to 4 kDa; The molecular weight of the bis(3-aminopropyl)-terminated polydimethylsiloxane is 1 to 5 kDa.
5. The preparation method according to claim 1, It is characterized in that The temperature of the first nucleophilic addition reaction is 70-90° C. and the time is 2-4 hours.
6. The preparation method according to claim 1, It is characterized in that The temperature of the second nucleophilic addition reaction is 20-30° C. and the time is 20-30 hours.
7. The preparation method according to claim 1, It is characterized in that The cross-linking polymerization reaction is carried out at a temperature of 20 to 30° C. and for a time of 4 to 8 hours.
8. The preparation method according to claim 1, It is characterized in that The organic solvent includes one or more of N,N-dimethylacetamide, chlorobenzene, fluorobenzene, tetrahydrofuran and 1,4-dioxane.
9. Perfluoropolyether-based polyurethane urea elastomer obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the perfluoropolyether-based polyurethane urea elastomer according to claim 9 in sealing materials.
Citation Information
Patent Citations
End-perfluoroalkyl and side-chain perfluoroalkyl double-modified polyurethane emulsion and preparation method thereof
CN109749048A
Multi-block polyamide-perfluoropolyether elastomer and preparation method thereof
CN117887022A
Fluorine containing polyurethane material and preparation method thereof
CN1371927A
Low temperature segmented copolymer compositions and methods
US8957175B1
Cited By
In-chain functionalized perfluoropolyether and preparation method thereof
CN119264408A
Underwater adhesive as well as preparation method and small molecule driven bonding method thereof
CN120665552A