Low-temperature electrolyte containing double solvents and application of low-temperature electrolyte in lithium-sulfur battery
By using a mixed electrolyte of weak coordination and high dielectric constant solvent in lithium-sulfur batteries, the problems of ion migration and diffusion in lithium-sulfur batteries at low temperatures were solved, and the stability and cycle performance of the batteries at extremely low temperatures were improved.
Patent Information
- Application Number
- CN202410936328.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
At low temperatures, lithium-sulfur batteries face challenges such as reduced ion migration rate, increased electrolyte/electrode interface impedance, and decreased ionic conductivity due to increased electrolyte viscosity. Existing electrolyte designs struggle to balance desolvation kinetics and ion diffusion rate at low temperatures.
A mixed electrolyte consisting of a weakly coordinating solvent and a high dielectric constant solvent is used. The weakly coordinating solvent reduces the desolvation energy of lithium ions, while the high dielectric constant solvent compensates for the insufficient ion migration rate, thus synergistically improving the ion diffusion kinetics at low temperatures.
This study improved the cycle performance of lithium-sulfur batteries at ultra-low temperatures, significantly accelerated low-temperature kinetics, and enhanced battery stability and cycle life.
Smart Images

Figure HDA0004941435360000011 
Figure HDA0004941435360000012 
Figure HDA0004941435360000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolyte preparation, and in particular to a preparation method and application of a weakly solvated electrolyte containing a weakly coordinating solvent, a high dielectric constant solvent and a lithium salt for improving the performance of a low-temperature lithium-sulfur battery. Background Art
[0002] The research background of low-temperature lithium-sulfur batteries involves the demand for rechargeable batteries that can work effectively under extremely low temperature conditions. Such batteries have important application value in special fields such as polar exploration, deep-sea operations, space missions and defense industry. Lithium-sulfur batteries are considered to be one of the most promising candidates due to their high energy density, low cost and environmental protection characteristics. The electrolyte plays a vital role in lithium-sulfur batteries. It not only acts as an ion conductor, but also widely participates in the conversion reaction of lithium and sulfur. The design of the electrolyte directly affects the cycle life, Coulombic efficiency and stability of the battery. However, at low temperatures, the main challenges faced by lithium-sulfur batteries include reduced ion migration rate, increased electrolyte / electrode interface impedance, and increased electrolyte viscosity leading to reduced ion conductivity. In recent years, researchers have conducted in-depth research on electrolyte solvents, lithium salts and additives, developed a variety of electrolyte formulations, and made significant progress. Generally, the choice of solvent is determined by two most important parameters: dielectric constant and donor number DN. Since desolvation is slow at low temperatures, it is advisable to select organic solvents with weak coordination to promote lithium ion desolvation through weak solvation, thereby accelerating low-temperature kinetics, but at the expense of ion diffusion in the bulk electrolyte. Therefore, the introduction of a suitable dual solvent to stimulate the competition between the desolvation kinetics and ion diffusion rate at low temperatures has attracted widespread attention. Summary of the invention
[0003] The use of weakly coordinated electrolytes improves the low-temperature performance of lithium-sulfur batteries. The main reason is that the addition of weakly coordinated solvents reduces the desolvation energy of lithium ions at low temperatures. The addition of high dielectric constant solvents can make up for the lack of ion migration rate in bulk electrolytes and improve the ion diffusion kinetics at low temperatures. The synergistic effect of the two is conducive to achieving the cycle performance of lithium-sulfur batteries at ultra-low temperatures. In this process, the type and content of weakly coordinated solvents and high dielectric constant solvents are crucial to the final cycle performance effect. Therefore, the present application discloses a preparation method and application of a weakly solvating lithium-sulfur battery electrolyte, using one or more of sulfolane (SUL), dimethoxymethane (DMM), dimethoxyethane (DME), ethylene glycol ethyl ether (2-Ethoxyethanol), ethylene glycol dibutyl ether (DEBGE), isopropyl ether, (DPE) butyl lactate (Butyl lactate), ethyl ether (Et2O), acetone (Acetone), ethyl acetate (EAC), n-propyl ether, tetrahydrofuran (THF), dimethyltetrahydrofuran (MeTHF), and methyl trifluoroacetate (MTFA). The addition of a weakly coordinating solvent reduces the desolvation energy of lithium ions at low temperatures. High dielectric constant solvents include one or more of acetonitrile (AN), pyridine (Py), 2-Fluoropyridin, dimethyl sulfoxide (DMSO), butyrolactone (BL), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), trimethyl phosphate (TMP), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), and butyl acetate (BA). The addition of high dielectric constant solvents can make up for the lack of ion migration rate in bulk electrolytes, improve ion diffusion kinetics at low temperatures, and effectively balance the competition between the solvation kinetics and ion diffusion rate at low temperatures. This weakly coordinated electrolyte has broad application prospects in the low-temperature electrolyte industry for lithium-sulfur batteries.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] The invention provides a method for preparing a low-temperature lithium-sulfur battery electrolyte containing a double solvent, comprising: dissolving a lithium salt in a mixed solvent consisting of a weakly coordinated solvent and a high dielectric constant solvent to obtain a weakly coordinated lithium-sulfur battery electrolyte.
[0006] In the weakly coordinated electrolyte of the lithium-sulfur battery, the lithium salt concentration is 0.5M to 5M; in the mixed solvent: the volume proportion of the weakly coordinated solvent is 10% to 90%, and the volume proportion of the high dielectric constant solvent is 10% to 90%.
[0007] Further, in the lithium-sulfur battery electrolyte, the weakly coordinated solvent is at least one of the following compounds: sulfolane (SUL), dimethoxymethane (DMM), dimethoxyethane (DME), ethylene glycol ethyl ether (2-Ethoxyethanol), ethylene glycol dibutyl ether (DEBGE), isopropyl ether, (DPE) butyl lactate (Butyl lactate), ethyl ether (Et2O), acetone (Acetone), ethyl acetate (EAC), n-propyl ether, tetrahydrofuran (THF), dimethyltetrahydrofuran (MeTHF), methyl trifluoroacetate (MTFA). In the lithium-sulfur battery weakly coordinated electrolyte, preferably, the volume proportion of the weakly coordinated solvent is 10% to 90%, and further, the volume proportion of the weakly coordinated solvent is 60% to 90%.
[0008] Further, the lithium-ion battery electrolyte also includes a lithium salt, and the lithium salt includes one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium nitrate (LiNO3), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium difluorooxalate borate (LiDFOB), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisfluorosulfonyl imide (LiFSI), lithium perchlorate (LiClO4), and lithium bisoxalate borate (LiBOB). Preferably, the total amount of lithium salt added is 0.5M-5M, and further, the total amount of lithium salt added is 1M-2M.
[0009] Further, the high dielectric constant electrolyte includes one or more of acetonitrile (AN), pyridine (Py), 2-fluoropyridine (2-Fluoropyridin), dimethyl sulfoxide (DMSO), butyrolactone (BL), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), trimethyl phosphate (TMP), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), and butyl acetate (BA). In the weakly coordinated electrolyte for lithium-sulfur batteries, preferably, the volume proportion of the high dielectric constant solvent is 10% to 90%, and further, the volume proportion of the high dielectric constant solvent is 10% to 40%.
[0010] The raw materials involved in the above-mentioned preparation method for lithium-sulfur battery electrolyte are all commercially available, and the equipment and processes used are well known to those skilled in the art.
[0011] The advantages and positive effects of the present invention are:
[0012] 1. The method of the present invention has low cost, simple operation and safe drug ingredients.
[0013] 2. The addition of a weakly coordinated solvent in the lithium-sulfur battery of the present invention reduces the desolvation energy of lithium ions at low temperatures, and the addition of a high dielectric constant solvent can make up for the insufficient ion migration rate in the bulk electrolyte and improve the ion diffusion kinetics at low temperatures. The synergistic effect of the two is conducive to achieving the cycle performance of lithium-sulfur batteries at ultra-low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The time-voltage diagram of the lithium-lithium symmetric battery of Example 1 and the comparative sample at -40°C;
[0015] Figure 2 The charge and discharge cycle curves of the full battery of Example 1 and the comparative sample at -40°C;
[0016] Figure 3 The time-voltage diagram of the lithium-lithium symmetric battery of Example 2 and the comparative sample at -40°C;
[0017] Figure 4 The charge and discharge cycle curves of the full battery of Example 2 and the comparison sample at -40°C. DETAILED DESCRIPTION
[0018] The following is further described in conjunction with specific examples. It should be understood that these examples are used to illustrate the present invention but not to limit the scope of the present invention. The implementation conditions used in the examples can be further adjusted according to specific construction conditions, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0019] Example 1
[0020] A method for preparing a lithium-sulfur battery electrolyte comprises: mixing dimethoxymethane and fluoroethylene carbonate (FEC) in a volume ratio of 5:5, adding 0.56 mg of lithium bis(fluorosulfonyl)imide (LiFSI) after mutual dissolution, and stirring until completely dissolved to obtain a weakly solvated lithium-sulfur electrolyte, wherein the concentration of lithium bis(fluorosulfonyl)imide (LiFSI) is 1 M.
[0021] Preparation method of comparative sample: 0.56 mg of lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in DME / DOL with a volume ratio of 1:1, and stirred until completely dissolved to obtain a lithium-sulfur battery electrolyte, and the concentration of lithium bis(fluorosulfonyl)imide (LiFSI) was 1M.
[0022] The prepared lithium-sulfur battery electrolyte was used to assemble a lithium-lithium symmetric battery. The time-voltage curve of the long cycle test at low temperature is shown in Figure 1 As shown, at -40°C, the current density is 0.1 mA / cm 2 , capacity is 0.1mAh / cm 2, and can maintain a stable cycle of 1100h and a polarization voltage of 0.15V, which can illustrate the stability of the electrolyte at low temperatures. It can be inferred that the low-temperature kinetics are significantly accelerated and the cycle life is improved.
[0023] Preparation method of positive electrode material: polyacrylonitrile and sublimed sulfur are ground for 30 minutes at a mass ratio of 1:4, and then transferred to a tube furnace for annealing at 450°C for 4 hours in an argon environment to obtain polypropylene sulfur. Polypropylene sulfur, conductive carbon black, and PVDF are mixed into a slurry at a mass ratio of 8:1:1, and then coated on a carbon-coated aluminum foil, and dried in a vacuum drying oven at 80°C for 12 hours to obtain a positive electrode sheet.
[0024] Full battery assembly method: Use polyacrylonitrile with a diameter of 10 mm as the positive electrode, a lithium sheet with a diameter of 16 mm as the negative electrode, celgard as the separator, drip the above-mentioned lithium-sulfur electrolyte, and package it under a pressure of 1.0T.
[0025] The full-battery lithium-sulfur battery prepared has a full-battery cycle stability test curve tested at low temperature as shown below: Figure 2 As shown in the figure, at -40°C and a current density of 0.25C, the capacity remains at a high discharge specific capacity of 480 mAh / g after 80 cycles, which indicates that the electrolyte still maintains good low-temperature cycle stability in the full battery. It can be inferred that the kinetics are significantly accelerated at low temperatures and the cycle life is improved.
[0026] Example 2
[0027] A method for preparing a lithium-sulfur battery electrolyte comprises: mixing ether and fluoroethylene carbonate (FEC) in a volume ratio of 3:7, adding 0.56 mg of lithium bis(fluorosulfonyl)imide (LiFSI) after mutual dissolution, and stirring until completely dissolved to obtain a weakly solvated lithium-sulfur electrolyte, wherein the concentration of lithium bis(fluorosulfonyl)imide (LiFSI) is 1.5 M.
[0028] Preparation method of comparative sample: 0.56 mg of lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in DME / DOL with a volume ratio of 1:1, and stirred until completely dissolved to obtain a lithium-sulfur battery electrolyte, and the concentration of lithium bis(fluorosulfonyl)imide (LiFSI) was 1.5 M.
[0029] The prepared lithium-sulfur battery electrolyte was used to assemble a lithium-lithium symmetric battery. The time-voltage curve of the long cycle test at low temperature is shown in Figure 3 As shown, at -40°C, the current density is 0.1 mA / cm 2 , capacity is 0.1mAh / cm 2 , and can maintain a stable cycle of 1580h and a polarization voltage of 0.18V, which can illustrate the stability of the electrolyte at low temperatures. It can be inferred that the low-temperature kinetics are significantly accelerated and the cycle life is improved.
[0030] Preparation method of positive electrode material: polyacrylonitrile and sublimed sulfur are ground for 30 minutes at a mass ratio of 1:4, and then transferred to a tube furnace for annealing at 450°C for 4 hours in an argon environment to obtain polypropylene sulfur. Polypropylene sulfur, conductive carbon black, and PVDF are mixed into a slurry at a mass ratio of 8:1:1, and then coated on a carbon-coated aluminum foil, and dried in a vacuum drying oven at 80°C for 12 hours to obtain a positive electrode sheet.
[0031] Full battery assembly method: Use polyacrylonitrile with a diameter of 10 mm as the positive electrode, a lithium sheet with a diameter of 16 mm as the negative electrode, celgard as the separator, drip the above-mentioned lithium-sulfur electrolyte, and package it under a pressure of 1.0T.
[0032] The full-battery lithium-sulfur battery prepared has a full-battery cycle stability test curve tested at low temperature as shown below: Figure 4 As shown in the figure, at -40°C and a current density of 0.25C, the capacity remains at a high discharge specific capacity of 450mAh / g after 80 cycles, which indicates that the electrolyte still maintains good low-temperature cycle stability in the full battery. It can be inferred that the kinetics are significantly accelerated at low temperatures and the cycle life is improved.
[0033] The above contents are further detailed descriptions of the invention in combination with specific embodiments, and it cannot be determined that the specific implementation of the invention is limited to these descriptions. For those skilled in the art of the present invention, any obvious simple deduction or replacement without departing from the concept of the present invention is within the scope of protection of the present invention.
Claims
1. A method for preparing a low-temperature electrolyte containing a dual solvent, characterized in that: include: Dissolving a lithium salt in a mixed solvent consisting of a weakly coordinated solvent and a high dielectric constant solvent to obtain a weakly solvated lithium-sulfur battery electrolyte; In the weakly coordinated electrolyte of the lithium-sulfur battery, the lithium salt concentration is 0.5M to 5M; in the mixed solvent: the volume proportion of the weakly coordinated solvent is 10% to 90%, and the volume proportion of the high dielectric constant solvent is 10% to 90%.
2. The preparation method according to claim 1, characterized in that: The weakly coordinated solvent component of the lithium-sulfur battery electrolyte is at least one of the following compounds: sulfolane (SUL), dimethoxymethane (DMM), dimethoxyethane (DME), ethylene glycol ethyl ether (2-Ethoxyethanol), ethylene glycol dibutyl ether (DEBGE), isopropyl ether, (DPE) butyl lactate (Butyllactate), ethyl ether (Et2O), acetone (Acetone), ethyl acetate (EAC), n-propyl ether (n-propyl ether), tetrahydrofuran (THF), dimethyltetrahydrofuran (MeTHF), methyl trifluoroacetate (MTFA) or more.
3. The preparation method according to claim 1, characterized in that: The lithium salt includes one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium nitrate (LiNO3), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), lithium difluorooxalatoborate (LiDFOB), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisfluorosulfonyl imide (LiFSI), lithium perchlorate (LiClO4), and lithium bisoxalatoborate (LiBOB).
4. The preparation method according to claim 1, characterized in that: The high dielectric constant solvent includes one or more of acetonitrile (AN), pyridine (Py), 2-fluoropyridine (2-Fluoropyridin), dimethyl sulfoxide (DMSO), butyrolactone (BL), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methylpropyl carbonate (MPC), trimethyl phosphate (TMP), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), and butyl acetate (BA).
5. The preparation method according to claim 1, characterized in that: In the weakly coordinated electrolyte of lithium-sulfur batteries, the lithium salt concentration is 1M-2M.
6. The preparation method according to claim 1, characterized in that: In the mixed solvent, the volume proportion of the weakly coordinating solvent is 60% to 90%.
Citation Information
Cited By
Binary solvent electrolyte and application thereof
CN121885779A
Binary solvent electrolyte and application thereof
CN121885779B