Bandage capable of promoting wound healing and containing stem cell exosome coating and preparation process of bandage
By covering the stem cell-containing exosome coating on the surface of the bandage, combining graft modification of composite hydrogel and polypropylene spun-optic elastic nonwoven materials, the shortcomings of existing bandages in wound healing are solved, and the rapid wound surface is achieved Healing and long-term functional recovery.
Patent Information
- Application Number
- CN202410981793.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
Existing bandages have limited effectiveness in promoting wound healing and cannot effectively assist wound healing.
Using a bandage containing stem cell exosome coating, it is coated on the surface of polypropylene spun-vinyl elastic nonwoven material after being compounded with a composite hydrogel. The biologically active substances of fat stem cell exosomes are used to promote wound healing, and spinning through polypropylene Surface grafting modification of viscoelastic nonwoven materials enhances binding force.
Effective healing of wounds is achieved, and by continuously releasing fat stem cell exosomes, it reduces the inflammatory response, promotes granulation tissue growth and new blood vessel formation, shortens wound healing time, and provides antibacterial effects.
Smart Images

Figure CN118903519A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of bandages, and in particular to a bandage containing a stem cell exosome coating for promoting wound healing and a preparation process thereof. Background Art
[0002] A bandage is a gauze strip used to wrap wounds or affected areas. It is a common medical supply and comes in many different types and multiple bandaging methods. You need to choose the appropriate type and bandaging method based on the injured area.
[0003] Bandages can be used to compress bleeding points to prevent bleeding. Bandages can be divided into 100% cotton plain bandages, wrinkled elastic bandages, spandex elastic bandages, PBT elastic bandages, cotton gauze woven bandages, viscose plaster bandages, and polypropylene spunbond elastic nonwoven bandages. Polypropylene spunbond elastic nonwoven bandages are soft and highly elastic, and are mainly used for surgical dressing care.
[0004] The existing bandage can only stop bleeding, but does not play a significant auxiliary role in wound healing.
[0005] Adipose-Derived Stem Cell Der ived Exosomes (ADSC-Exos) are tiny vesicles secreted by stem cells in adipose tissue, with a diameter usually between 30 and 150 nanometers. The outer layer of these tiny vesicles is composed of a lipid bilayer, and the interior contains a variety of biologically active substances, such as proteins and nucleic acids. These substances give adipose-derived stem cell exosomes unique biological functions and effects.
[0006] Adipose stem cells can participate in tissue repair and regeneration: Studies have shown that adipose stem cell exosomes can promote the repair and regeneration of damaged tissues. They can participate in the process of wound healing and tissue regeneration by regulating inflammatory responses, accelerating cell proliferation and differentiation, and promoting angiogenesis. In addition, adipose stem cell exosomes can also inhibit scar formation and improve the appearance and function of the wound surface.
[0007] Based on this, a bandage containing a stem cell exosome coating that promotes wound healing is provided to solve existing technical problems. Summary of the invention
[0008] The purpose of the present invention is to provide a bandage containing a stem cell exosome coating for promoting wound healing, so as to solve the deficiencies in the prior art.
[0009] The technical solution adopted by the present invention is as follows:
[0010] A bandage containing a stem cell exosome coating for promoting wound healing, wherein the surface of the bandage is covered with a layer of stem cell exosome coating;
[0011] The stem cell exosomes are compounded with the composite hydrogel and then covered on the surface of the bandage;
[0012] The stem cell exosome coating is specifically covered on one side of the bandage;
[0013] The bandage is based on polypropylene spunbond elastic nonwoven material, which is obtained after surface grafting modification and then cutting.
[0014] As a further technical solution: the composite hydrogel preparation method is:
[0015] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0016] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0017] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0018] Add the acryloyl chloride solution dropwise to the first mixed solution, adjust the temperature to 60-62°C under inert atmosphere protection, keep stirring for 5 minutes, then adjust the pH of the system to 9.0, continue stirring and reacting for 3-4 hours, then discharge the material, remove tetrahydrofuran by rotary evaporation, extract with ethyl acetate, and obtain the composite monomer after drying;
[0019] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0020] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0021] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0022] As a further technical solution: the mixing ratio of the sodium hydroxide and deionized water is 15-16g:100mL;
[0023] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:100-110mL;
[0024] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0025] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0026] The inert gas is a nitrogen atmosphere.
[0027] As a further technical solution: the mixing ratio of the tannic acid and deionized water is 1-2 g: 10 mL;
[0028] The mass ratio of tannic acid to composite monomer is 1:22-25;
[0029] The mixing mass ratio of the phenyldione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0030] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0031] As a further technical solution: the UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0032] As a further technical solution: the bandage containing stem cell exosome coating that promotes wound healing has a thickness of 130-140 μm;
[0033] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5-6 μm.
[0034] As a further technical solution: the surface grafting modification method of the polypropylene spunbond elastic nonwoven material is:
[0035] First, chitosan solution and glutaraldehyde solution are prepared;
[0036] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0037] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0038] As a further technical solution: the chitosan solution has a mass fraction of 8-9%;
[0039] The mass fraction of the glutaraldehyde solution is 8-9%;
[0040] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0041] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0042] The vacuum degree of vacuum impregnation is 0.1Pa;
[0043] The vacuum drying temperature was 50°C and the time was 4 hours.
[0044] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0045] (1) preparing composite hydrogel;
[0046] (2) Prepare adipose stem cell exosome suspension;
[0047] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0048] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0049] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0050] Beneficial effects:
[0051] The bandage prepared by the present invention can not only directly compress the wound surface by applying pressure, but also, when the bandage is tightly wrapped around the wound, it will generate a certain pressure on the blood vessels around the wound. This pressure can promote the aggregation of platelets on the blood vessel wall and release coagulation factors, thereby starting the coagulation process. At the same time, the pressure can also squeeze the blood vessels to shrink or occlude them, reduce blood outflow, and achieve the purpose of hemostasis.
[0052] The bandage prepared by the present invention also plays a role in protecting the wound during the process of hemostasis. Through tight bandaging, the bandage can isolate the invasion of external bacteria and other pollutants, thereby reducing the risk of infection.
[0053] After bandaging, a stable environment is formed. In this stable environment, the wound can get sufficient rest and protection. Moreover, under the action of adipose stem cell exosomes, it can promote the growth of granulation tissue and the repair of epithelial cells, providing good conditions for wound healing.
[0054] The present invention can reduce the inflammatory response by covering the bandage surface with a layer of stem cell exosome coating and continuously and slowly releasing adipose stem cell exosomes. This is because the inflammatory response is an indispensable stage in the wound healing process. However, excessive inflammatory response may lead to aggravated tissue damage and affect the healing process. The continuous action of adipose stem cell exosomes can inhibit the expression of inflammatory factors and reduce the degree of inflammatory response, thereby facilitating the healing of the wound.
[0055] The various angiogenic factors contained in the released adipose stem cell exosomes can promote the proliferation and migration of endothelial cells, accelerate the formation of new blood vessels, and provide sufficient nutrition and oxygen support to the wound, thereby promoting wound healing and shortening wound healing time.
[0056] In addition, certain components in adipose stem cell exosomes can regulate the activity of collagenase, promote the degradation and rearrangement of collagen, and make the extracellular matrix more orderly and stable, which is beneficial to the long-term healing of wounds and the recovery of function.
[0057] The composite hydrogel prepared by the present invention can be combined with adipose stem cell exosomes, so that when the bandage is used, it can continuously release adipose stem cell exosomes, thereby promoting window healing. By grafting and modifying the surface of the polypropylene spunbond elastic nonwoven material, it can not only better combine with the composite hydrogel, but also carry chitosan to play an antibacterial role. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 This is a bar graph of residual wound surface of Kunming mice after 5 days of experiment;
[0059] Figure 2 This is an electron micrograph of exosomes;
[0060] Figure 3 This is an electron micrograph of the composite gel. DETAILED DESCRIPTION
[0061] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0062] The method for preparing the adipose stem cell exosome suspension used in the following examples is as follows:
[0063] Adult adipose-derived stem cells were purchased from Saiye Biotechnology Co., Ltd. When the cell density was about 80%, they were cultured in a 37°C, 5% CO2 incubator using DMEM medium without exosomes for 48 hours, the supernatant culture fluid was collected, centrifuged at 3000g×10min, the supernatant culture fluid was taken, cells and cell debris were removed, the supernatant was centrifuged again at 6000g×15min, the supernatant was taken, and centrifuged again at 12000g×15min, the supernatant was discarded, the precipitate was retained, and PBS was added for re-suspending to obtain adipose-derived stem cell exosome suspension;
[0064] The exosome concentration was 1.35×10 7 Pieces / mL;
[0065] Example 1
[0066] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0067] (1) preparing composite hydrogel;
[0068] (2) Prepare adipose stem cell exosome suspension;
[0069] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0070] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0071] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0072] The preparation method of the composite hydrogel is as follows:
[0073] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0074] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0075] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0076] The acryloyl chloride solution was added dropwise to the first mixed solution, and the temperature was adjusted to 60° C. under the protection of an inert atmosphere, and the mixture was stirred for 5 minutes. Then, the pH of the system was adjusted to 9.0, and the reaction was continued with stirring for 3 hours. Then, the mixture was discharged, tetrahydrofuran was removed by rotary evaporation, and then ethyl acetate was used for extraction. After drying, the composite monomer was obtained.
[0077] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0078] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0079] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0080] The mixing ratio of sodium hydroxide and deionized water is 15g:100mL;
[0081] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:100mL;
[0082] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0083] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0084] The inert gas is a nitrogen atmosphere.
[0085] The mixing ratio of tannic acid and deionized water is 1g:10mL;
[0086] The mass ratio of tannic acid to composite monomer is 1:22;
[0087] The mixing mass ratio of the phenyldione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0088] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0089] UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0090] The bandage coated with stem cell exosomes that promote wound healing has a thickness of 130 μm;
[0091] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5 μm.
[0092] The surface grafting modification method of polypropylene spunbond elastic nonwoven material is as follows:
[0093] First, chitosan solution and glutaraldehyde solution are prepared;
[0094] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0095] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0096] The mass fraction of chitosan solution is 8%;
[0097] The mass fraction of the glutaraldehyde solution is 8%;
[0098] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0099] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0100] The vacuum degree of vacuum impregnation is 0.1Pa;
[0101] The vacuum drying temperature was 50°C and the time was 4 hours.
[0102] Example 2
[0103] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0104] (1) preparing composite hydrogel;
[0105] (2) Prepare adipose stem cell exosome suspension;
[0106] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0107] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0108] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0109] The preparation method of the composite hydrogel is as follows:
[0110] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0111] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0112] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0113] The acryloyl chloride solution was added dropwise to the first mixed solution, and the temperature was adjusted to 61° C. under the protection of an inert atmosphere, and the mixture was stirred for 5 minutes. Then, the pH of the system was adjusted to 9.0, and the reaction was continued with stirring for 3.5 hours. Then, the mixture was discharged, tetrahydrofuran was removed by rotary evaporation, and then ethyl acetate was used for extraction. After drying, the composite monomer was obtained.
[0114] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0115] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0116] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0117] The mixing ratio of sodium hydroxide and deionized water is 15.2g:100mL;
[0118] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:103mL;
[0119] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0120] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0121] The inert gas is a nitrogen atmosphere.
[0122] The mixing ratio of tannic acid and deionized water is 1.2 g:10 mL;
[0123] The mass ratio of tannic acid to composite monomer is 1:23;
[0124] The mixing mass ratio of the phenyl dione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0125] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0126] UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0127] The bandage coated with stem cell exosomes that promote wound healing has a thickness of 130 μm;
[0128] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5.2 μm.
[0129] The surface grafting modification method of polypropylene spunbond elastic nonwoven material is as follows:
[0130] First, chitosan solution and glutaraldehyde solution are prepared;
[0131] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0132] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0133] The mass fraction of chitosan solution is 8.3%;
[0134] The mass fraction of the glutaraldehyde solution is 8.3%;
[0135] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0136] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0137] The vacuum degree of vacuum impregnation is 0.1Pa;
[0138] The vacuum drying temperature was 50°C and the time was 4 hours.
[0139] Example 3
[0140] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0141] (1) preparing composite hydrogel;
[0142] (2) Prepare adipose stem cell exosome suspension;
[0143] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0144] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0145] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0146] The composite hydrogel preparation method is as follows:
[0147] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0148] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0149] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0150] The acryloyl chloride solution was added dropwise to the first mixed solution, and the temperature was adjusted to 61° C. under the protection of an inert atmosphere, and the mixture was stirred for 5 minutes. Then, the pH of the system was adjusted to 9.0, and the reaction was continued with stirring for 4 hours. Then, the mixture was discharged, tetrahydrofuran was removed by rotary evaporation, and then ethyl acetate was used for extraction. After drying, the composite monomer was obtained.
[0151] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0152] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0153] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0154] The mixing ratio of sodium hydroxide and deionized water is 16g:100mL;
[0155] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:108mL;
[0156] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0157] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0158] The inert gas is a nitrogen atmosphere.
[0159] The mixing ratio of tannic acid and deionized water is 2 g:10 mL;
[0160] The mass ratio of tannic acid to composite monomer is 1:22;
[0161] The mixing mass ratio of the phenyldione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0162] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0163] UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0164] The bandage coated with stem cell exosomes that promote wound healing has a thickness of 130 μm;
[0165] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5.5 μm.
[0166] The surface grafting modification method of polypropylene spunbond elastic nonwoven material is as follows:
[0167] First, chitosan solution and glutaraldehyde solution are prepared;
[0168] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0169] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0170] The mass fraction of chitosan solution is 8.5%;
[0171] The mass fraction of the glutaraldehyde solution is 8.5%;
[0172] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0173] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0174] The vacuum degree of vacuum impregnation is 0.1Pa;
[0175] The vacuum drying temperature was 50°C and the time was 4 hours.
[0176] Example 4
[0177] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0178] (1) preparing composite hydrogel;
[0179] (2) Prepare adipose stem cell exosome suspension;
[0180] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0181] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0182] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0183] The composite hydrogel preparation method is as follows:
[0184] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0185] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0186] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0187] The acryloyl chloride solution was added dropwise to the first mixed solution, and the temperature was adjusted to 61°C under the protection of an inert atmosphere, and the mixture was stirred for 5 minutes. Then, the pH of the system was adjusted to 9.0, and the reaction was continued with stirring for 3 hours. Then, the mixture was discharged, tetrahydrofuran was removed by rotary evaporation, and then ethyl acetate was used for extraction. After drying, the composite monomer was obtained.
[0188] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0189] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0190] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0191] The mixing ratio of sodium hydroxide and deionized water is 15g:100mL;
[0192] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:106mL;
[0193] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0194] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0195] The inert gas is a nitrogen atmosphere.
[0196] The mixing ratio of tannic acid and deionized water is 1.8 g:10 mL;
[0197] The mass ratio of tannic acid to composite monomer is 1:24;
[0198] The mixing mass ratio of the phenyl dione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0199] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0200] UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0201] The bandage coated with stem cell exosomes that promote wound healing has a thickness of 130 μm;
[0202] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5.2 μm.
[0203] The surface grafting modification method of polypropylene spunbond elastic nonwoven material is as follows:
[0204] First, chitosan solution and glutaraldehyde solution are prepared;
[0205] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0206] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0207] The mass fraction of chitosan solution is 8.89%;
[0208] The mass fraction of the glutaraldehyde solution is 8.8%;
[0209] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0210] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0211] The vacuum degree of vacuum impregnation is 0.1Pa;
[0212] The vacuum drying temperature was 50°C and the time was 4 hours.
[0213] Example 5
[0214] A method for preparing a bandage containing a stem cell exosome coating for promoting wound healing comprises the following steps:
[0215] (1) preparing composite hydrogel;
[0216] (2) Prepare adipose stem cell exosome suspension;
[0217] (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite;
[0218] (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials;
[0219] (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
[0220] The composite hydrogel preparation method is as follows:
[0221] First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution;
[0222] Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution;
[0223] Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution;
[0224] The acryloyl chloride solution was added dropwise to the first mixed solution, and the temperature was adjusted to 62° C. under the protection of an inert atmosphere, and the mixture was stirred for 5 minutes. Then, the pH of the system was adjusted to 9.0, and the reaction was continued with stirring for 4 hours. Then, the mixture was discharged, tetrahydrofuran was removed by rotary evaporation, and then ethyl acetate was used for extraction. After drying, the composite monomer was obtained.
[0225] Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution;
[0226] Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution;
[0227] The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
[0228] The mixing ratio of sodium hydroxide and deionized water is 16g:100mL;
[0229] The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:110mL;
[0230] The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4;
[0231] The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100;
[0232] The inert gas is a nitrogen atmosphere.
[0233] The mixing ratio of tannic acid and deionized water is 2 g:10 mL;
[0234] The mass ratio of tannic acid to composite monomer is 1:25;
[0235] The mixing mass ratio of the phenyl dione and dimethyl sulfoxide is 0.01 g:0.2 mL;
[0236] The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
[0237] UV curing uses 400nm wavelength ultraviolet rays for curing, and the curing time is 5 minutes.
[0238] The bandage coated with stem cell exosomes that promote wound healing has a thickness of 130 μm;
[0239] The thickness of the stem cell-containing exosome coating that promotes wound healing is 5 μm.
[0240] The surface grafting modification method of polypropylene spunbond elastic nonwoven material is as follows:
[0241] First, chitosan solution and glutaraldehyde solution are prepared;
[0242] mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution;
[0243] Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
[0244] The mass fraction of chitosan solution is 9%;
[0245] The mass fraction of the glutaraldehyde solution is 9%;
[0246] The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1;
[0247] The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10;
[0248] The vacuum degree of vacuum impregnation is 0.1Pa;
[0249] The vacuum drying temperature was 50°C and the time was 4 hours.
[0250] Comparative Example 1
[0251] Based on Example 1, adipose stem cell exosomes are not added to the composite hydrogel, and the rest of the technical solutions remain unchanged.
[0252] Comparative Example 2
[0253] On the basis of Example 1, the polypropylene spunbond elastic nonwoven material is not subjected to graft modification treatment, and the rest of the technical scheme remains unchanged.
[0254] Comparative Example 3
[0255] On the basis of Example 1, the composite hydrogel was replaced with commercially available polyvinyl alcohol hydrogel, and the rest of the technical scheme remained unchanged.
[0256] test:
[0257] Ninety Kunming mice, weighing 25 ± 1 g and aged 8 weeks, were randomly divided into 9 groups;
[0258] Each Kunming mouse was anesthetized by injection of pentobarbital at a dose of 45 mg / kg, and then the model was established: first, a piece of hair on the back of the Kunming mouse was shaved, and then a wound with a diameter of 20±1 mm was made on the back skin of the Kunming mouse with a sterile scalpel, and then wrapped with the same size of the embodiment and comparative bandages, respectively, leaving one group untreated, and comparing the wound healing conditions of each group after 5 days:
[0259] Table 1
[0260] Wound healing rate% Example 1 94.3 Example 2 95.2 Example 3 95.5 Example 4 95.1 Example 5 94.6 Comparative Example 1 60.3 Comparative Example 2 89.2 Comparative Example 3 84.9 Control group 45.6
[0261] It can be seen from Table 1 that the bandage prepared by the present invention has a high promoting effect on wound healing and can accelerate the healing of wounds.
[0262] The complete healing time of wounds in each group of the comparative example and comparative example:
[0263] Table 2
[0264] Complete wound healing time / day Example 1 9 Example 2 8 Example 3 8 Example 4 8 Example 5 9 Comparative Example 1 16 Comparative Example 2 11 Comparative Example 3 14 Control group 18
[0265] It can be seen from Table 2 that the bandage prepared by the method of the present invention has a strong wound healing promoting effect.
[0266] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.
Claims
1. A bandage containing a stem cell exosome coating for promoting wound healing, characterized in that: The surface of the bandage is covered with a coating layer containing stem cell exosomes; The stem cell exosomes are compounded with the composite hydrogel and then covered on the surface of the bandage; The stem cell exosome coating is specifically covered on one side of the bandage; The bandage is based on polypropylene spunbond elastic nonwoven material, which is obtained after surface grafting modification and then cutting.
2. A bandage containing stem cell exosome coating for promoting wound healing according to claim 1, characterized in that: The composite hydrogel preparation method is as follows: First, sodium hydroxide is added to deionized water, and the mixture is stirred to obtain a sodium hydroxide solution; Mix threonine and lysine, then add them into the sodium hydroxide solution, and stir and mix for 20 minutes to obtain a first mixed solution; Adding acryloyl chloride to anhydrous tetrahydrofuran, stirring and mixing evenly to obtain an acryloyl chloride solution; Add the acryloyl chloride solution dropwise to the first mixed solution, adjust the temperature to 60-62°C under inert atmosphere protection, keep stirring for 5 minutes, then adjust the pH of the system to 9.0, continue stirring and reacting for 3-4 hours, then discharge the material, remove tetrahydrofuran by rotary evaporation, extract with ethyl acetate, and obtain the composite monomer after drying; Add tannic acid to deionized water, stir and mix evenly to obtain a tannic acid solution; Add phenyl dione to dimethyl sulfoxide, stir and mix well to obtain a phenyl dione solution; The tannic acid solution was mixed with the composite monomer, then added dropwise into the phenyldione solution, subjected to ultrasonic dispersion for 10 minutes, and then subjected to UV curing to obtain a composite hydrogel.
3. A bandage containing stem cell exosome coating for promoting wound healing according to claim 2, characterized in that: The mixing ratio of the sodium hydroxide and deionized water is 15-16 g: 100 mL; The mixing ratio of amino acid, lysine and sodium hydroxide solution is 6g:6g:100-110mL; The volume ratio of acryloyl chloride and anhydrous tetrahydrofuran is 5:4; The mixing volume ratio of the acryloyl chloride solution and the first mixed solution is 31:100; The inert gas is a nitrogen atmosphere.
4. A bandage containing stem cell exosome coating for promoting wound healing according to claim 2, characterized in that: The mixing ratio of the tannic acid and deionized water is 1-2 g: 10 mL; The mass ratio of tannic acid to composite monomer is 1:22-25; The mixing mass ratio of the phenyl dione and dimethyl sulfoxide is 0.01 g:0.2 mL; The volume ratio of the phenyldione solution to the tannic acid solution is 0.18 mL:9 mL.
5. A bandage containing stem cell exosome coating for promoting wound healing according to claim 2, characterized in that: The UV curing is performed using ultraviolet light with a wavelength of 400 nm, and the curing time is 5 minutes.
6. A bandage containing stem cell exosome coating for promoting wound healing according to claim 1, characterized in that: The bandage containing stem cell exosome coating that promotes wound healing has a thickness of 130-140 μm; The thickness of the stem cell-containing exosome coating that promotes wound healing is 5-6 μm.
7. A bandage containing stem cell exosome coating for promoting wound healing according to claim 1, characterized in that: The surface grafting modification method of the polypropylene spunbond elastic nonwoven material is as follows: First, chitosan solution and glutaraldehyde solution are prepared; mixing the chitosan solution with the glutaraldehyde solution to obtain a grafting solution; Add the polypropylene spunbond elastic nonwoven material and the grafting liquid into a vacuum impregnation reactor, adjust the temperature to 50°C, keep warm and stir for 4 hours, then take it out, dry it with hot air at 60°C for 30 minutes, then wash it with 50% ethanol solution and deionized water, and then vacuum dry it.
8. A bandage containing stem cell exosome coating for promoting wound healing according to claim 7, characterized in that: The mass fraction of the chitosan solution is 8-9%; The mass fraction of the glutaraldehyde solution is 8-9%; The chitosan solution and the glutaraldehyde solution were mixed in a mass ratio of chitosan to glutaraldehyde of 1:1; The mixing ratio of polypropylene spunbond elastic nonwoven material and grafting liquid is 1:10; The vacuum degree of vacuum impregnation is 0.1Pa; The vacuum drying temperature was 50°C and the time was 4 hours.
9. The method for preparing a bandage containing a stem cell exosome coating for promoting wound healing according to claim 1, characterized in that: The following steps are involved: (1) preparing composite hydrogel; (2) Prepare adipose stem cell exosome suspension; (3) adding the composite hydrogel to the adipose stem cell exosome suspension at a mass ratio of 1:5, immersing the suspension at 10° C. for 2 hours, and then taking it out to obtain a composite; (4) Surface grafting modification of polypropylene spunbond elastic nonwoven materials; (5) The composite is combined with a polypropylene spunbond elastic nonwoven material to graft and modify one side of the surface to form a stem cell exosome coating.
Citation Information
Cited By
Mesenchymal stem cell exosome in-vitro dressing as well as preparation method and application thereof
CN120078924A
An external application dressing of mesenchymal stem cell exosomes, its preparation method and application
CN120078924B