High-entropy alloy and preparation method thereof

Through the preparation method of specific element composition and high-entropy alloy, the problem of insufficient performance in the alloy during hydrogen adsorption and release is solved, and efficient hydrogen storage performance is achieved, especially the improvement of hydrogen absorption and hydrogen release cycle performance under room temperature conditions. .

CN118910486APending Publication Date: 2024-11-08CHINA INSTITUTE OF ATOMIC ENERGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410985594.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There are many problems in the hydrogen adsorption and release process of existing alloys, which limit their application as hydrogen storage material, especially the poor performance of hydrogen absorption and hydrogen release circulation under room temperature conditions, and the hydrogen storage capacity is low.

Method used

Using high-entropy alloys composed of specific elements, Ti, V, Zr, Nb and Hf, through pretreatment and environmental processing of smelting equipment, ensure uniform distribution of elements, and prepare high-entropy that can absorb hydrogen at room temperature and release hydrogen at 600°C. Alloys and achieve high purity and uniform distribution through high vacuum arc smelting and casting techniques.

Benefits of technology

It realizes efficient hydrogen absorption and hydrogen discharge cycle under room temperature conditions, with high hydrogen storage capacity (>1.6 wt.%) and excellent hydrogen absorption kinetics. The maximum hydrogen storage volume remains at 95% after 3 hydrogen absorption and discharge cycles. above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910486A_ABST
    Figure CN118910486A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the field of alloy smelting by adopting a smelting method, in particular to a high-entropy alloy and a preparation method thereof.According to the high-entropy alloy, due to the fact that specific elements are adopted, and the specific matching range is adopted for all the elements, when the high-entropy alloy is adopted for hydrogen storage, the hydrogen storage efficiency is improved, and the hydrogen storage efficiency is improved. Hydrogen can be absorbed at room temperature, and hydrogen desorption circulation at 600 DEG C can be realized; activation is easy, and activation can be achieved through one-time hydrogen absorption and one-time hydrogen desorption; the hydrogen storage capacity is high (greater than 1.6 wt.%); the hydrogen absorption and desorption cycle performance is good, the hydrogen absorption kinetics is excellent, the maximum hydrogen absorption amount can be rapidly achieved, and the maximum hydrogen storage amount is kept at 95% or above after three times of hydrogen absorption and desorption cycles. According to the preparation method of the high-entropy alloy, preparation of the high-entropy alloy can be achieved, all the elements are evenly distributed in the smelting process through pretreatment of the raw materials and treatment of the smelting environment, and therefore the high-entropy alloy with the high purity and the evenly-distributed elements can be prepared through the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the field of alloy smelting using a smelting method, and in particular, to a high entropy alloy and a preparation method thereof. Background Art

[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0003] Hydrogen can be adsorbed into the gaps of alloys under certain hydrogen pressure and temperature to form metal hydrides. When heated, the hydrogen in the metal hydrides can be released. However, current alloys have many problems in the process of hydrogen adsorption or release, which limits the application of alloys as hydrogen storage materials. Summary of the invention

[0004] A brief overview of the present application is provided below in order to provide a basic understanding of certain aspects of the present application. It should be understood that this overview is not an exhaustive overview of the present application. It is not intended to identify the key or important parts of the present application, nor is it intended to limit the scope of the present application. Its purpose is merely to present certain concepts in a simplified form as a prelude to a more detailed description discussed later.

[0005] One aspect of the present application provides a high entropy alloy, which includes the following elements: Ti, V, Zr, Nb and Hf, wherein the percentage of the atomic content of each element satisfies the following range: 23%≤Ti≤27%, 26%≤V≤30%, 17%≤Zr≤25%, 16%≤Nb≤22%, 0%≤Hf≤18%, and the sum of the atomic content of the above elements is 100%.

[0006] Another aspect of the present application provides a method for preparing the aforementioned high entropy alloy, which comprises the following steps: S1: pretreating the raw materials for preparing the high entropy alloy; S2: weighing the pretreated raw materials according to the proportions of the components of the high entropy alloy; S3: placing the weighed raw materials into a smelting equipment to be used for preparing the high entropy alloy; S4: treating the internal environment of the smelting equipment to remove oxygen; S5: melting and cooling the raw materials into alloy ingots in the smelting equipment; S6: treating the alloy ingot to obtain a melt in which the elements constituting the high entropy alloy are evenly distributed, and casting the high entropy alloy after the alloy is completely melted.

[0007] The high entropy alloy of the present application uses specific elements and adopts a specific ratio range for each element, so that when the high entropy alloy is used for hydrogen storage, it can absorb hydrogen at room temperature and release hydrogen at 600°C in a cycle; it is easy to activate, and activation is achieved by one hydrogen absorption and one hydrogen release; it has a high hydrogen storage capacity (>1.6wt.%); it has good hydrogen absorption and desorption cycle performance, excellent hydrogen absorption kinetics, and can quickly reach the maximum hydrogen absorption amount. After three hydrogen absorption and desorption cycles, the maximum hydrogen storage amount is maintained at more than 95%.

[0008] The high entropy alloy preparation method provided in the present application can realize the preparation of the above-mentioned high entropy alloy by pretreating the raw materials, treating the smelting environment and making the various elements evenly distributed during the smelting process. Thus, by using the above method, a high entropy alloy with high purity and uniform distribution of various elements can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] In order to further illustrate the above and other advantages and features of the present application, the specific embodiments of the present application are further described in detail below in conjunction with the accompanying drawings. The accompanying drawings together with the following detailed description are included in this specification and form a part of this specification. Elements with the same function and structure are represented by the same reference numerals. It should be understood that these drawings only describe typical examples of the present application and should not be regarded as limiting the scope of the present application.

[0010] Figure 1 The Ti prepared in Examples 1 and 2 25 V 28 Zr 24 Nb 23 and Ti 24 V 26 Zr 17 Nb 16 Hf 17 X-ray diffraction (XRD) pattern of high entropy alloy before hydrogen absorption test.

[0011] Figure 2 The Ti prepared in Example 1 25 V 28 Zr 24 Nb 23 Hydrogen absorption kinetic curve of high entropy alloy at 20℃ and 0.2MPa hydrogen pressure.

[0012] Figure 3 The Ti prepared in Example 1 25 V 28 Zr 24 Nb 23 Pressure-concentration-temperature (PCT) curves of hydrogen absorption of high entropy alloys at 20°C.

[0013] Figure 4The Ti prepared in Example 1 25 V 28 Zr 24 Nb 23 Hydrogen absorption kinetic curves of high entropy alloy after three cycles of hydrogen absorption and desorption at 20℃ and 0.2MPa hydrogen pressure.

[0014] Figure 5 The Ti prepared in Example 2 24 V 26 Zr 17 Nb 16 Hf 17 Hydrogen absorption kinetic curve of high entropy alloy at 20℃ and 0.2MPa hydrogen pressure.

[0015] Figure 6 The Ti prepared in Example 2 24 V 26 Zr 17 Nb 16 Hf 17 Pressure-concentration-temperature (PCT) curves of hydrogen absorption of high entropy alloys at 20°C.

[0016] Figure 7 The Ti prepared in Example 2 24 V 26 Zr 17 Nb 16 Hf 17 Hydrogen absorption kinetic curves of high entropy alloy after three cycles of hydrogen absorption and desorption at 20℃ and 0.2MPa hydrogen pressure. DETAILED DESCRIPTION

[0017] Exemplary embodiments of the present application will be described below in conjunction with the accompanying drawings. For the sake of clarity and conciseness, not all features of the actual implementation are described in the specification. However, it should be understood that many implementation-specific decisions must be made in the process of developing any such actual implementation in order to achieve the developer's specific goals, such as meeting those constraints related to the system and business, and these constraints may vary from implementation to implementation. In addition, it should be understood that although the development work may be very complex and time-consuming, it is only a routine task for those skilled in the art who benefit from the content of this application.

[0018] It is also necessary to explain here that, in order to avoid obscuring the present application due to unnecessary details, only the device structure and / or processing steps closely related to the scheme according to the present application are shown in the accompanying drawings, while other details that are not very relevant to the present application are omitted.

[0019] The disclosure below provides a plurality of different embodiments or examples to implement the present application. In order to simplify the disclosure of the present application, the parts and methods of specific examples are described below. Of course, they are merely examples, and the purpose is not to limit the present application. In the description of the embodiments of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically limited.

[0020] The inventor of the present application has found that high entropy alloys can be used as solid hydrogen storage materials. High entropy alloys are generally melted from different elemental metal materials. The obtained high entropy alloys have different elements in their composition. Different elements cause the performance of the high entropy alloys to be different during use as solid hydrogen storage materials, especially the performance that is not conducive to being used as solid hydrogen storage materials. In addition, there is no general rule that can be followed for the performance of high entropy alloys obtained by including different elements that is not conducive to being used as solid hydrogen storage materials, and there is no combination of different elemental metal materials to obtain high entropy alloys that can meet the requirements of being used as solid hydrogen storage materials.

[0021] An embodiment of the present application proposes a high entropy alloy, which includes the following elements: Ti, V, Zr, Nb and Hf, wherein the percentage of the atomic content of each element satisfies the following range: 23%≤Ti≤27%, 26%≤V≤30%, 17%≤Zr≤25%, 16%≤Nb≤22%, 0%≤Hf≤18%, and the sum of the atomic content of the above elements is 100%.

[0022] The following expression can be used to represent the high entropy alloy of the present application: Ti a V b Zr c Nb d Hf e The subscripts a, b, c, d, and e in the above formula represent the content of the element in the alloy.

[0023] The high entropy alloy of the present application uses specific elements and adopts a specific ratio range for each element, so that when the high entropy alloy is used for hydrogen storage, it can absorb hydrogen at room temperature and release hydrogen at 600°C in a cycle; it is easy to activate, and activation is achieved by one hydrogen absorption and one hydrogen release; it has a high hydrogen storage capacity (>1.6wt.%); it has good hydrogen absorption and desorption cycle performance, excellent hydrogen absorption kinetics, and can quickly reach the maximum hydrogen absorption amount. After three hydrogen absorption and desorption cycles, the maximum hydrogen storage amount is maintained at more than 95%.

[0024] Another embodiment of the present application provides a method for preparing the aforementioned high entropy alloy, which comprises the following steps: S1: pretreating the raw materials for preparing the high entropy alloy; S2: weighing the pretreated raw materials according to the proportions of the components of the high entropy alloy; S3: placing the weighed raw materials into a smelting equipment to be used for preparing the high entropy alloy; S4: treating the internal environment of the smelting equipment to remove oxygen; S5: melting and cooling the raw materials into alloy ingots in the smelting equipment; S6: treating the alloy ingot to obtain a melt in which the elements constituting the high entropy alloy are evenly distributed, and casting the high entropy alloy after the alloy is completely melted.

[0025] The high entropy alloy preparation method provided in the present application can realize the preparation of the above-mentioned high entropy alloy by pretreating the raw materials, treating the smelting environment and making the various elements evenly distributed during the smelting process. Thus, by using the above method, a high entropy alloy with high purity and uniform distribution of various elements can be prepared.

[0026] In some embodiments, in step S1, the raw material of the high entropy alloy is polished and cleaned and dried to remove impurities. Through the above treatment, the purity of the raw material can be improved. For example, the raw material of the high entropy alloy can be polished with sandpaper to polish off the oxide layer on its surface; thereafter, the raw material is placed in an organic solution and cleaned with ultrasound, for example, in alcohol and acetone, and after cleaning, the raw material is dried. The residual substances produced by grinding on the surface of the raw material can be removed by cleaning and drying operations.

[0027] In step S2, raw materials of each element are weighed according to the atomic ratio of the elements contained in the high entropy alloy, and the total weight of the weighed raw materials is (100, weighed) g.

[0028] In step S3, weighed Ti, V, Zr, Nb and Hf are put into a crucible of a high vacuum arc melting furnace in order of melting points from low to high, with Ti having the lowest melting point at the bottom.

[0029] In step S4, the interior of the cavity of the high vacuum arc melting furnace is evacuated (e.g., to 5 Pa), and then high-purity (e.g., 99.999%) argon gas is introduced. The above operation is repeated several times until the vacuum degree reaches a certain value (e.g., 1×10 -3 Pa), and high-purity argon is introduced into the high vacuum arc melting furnace again, so that the pressure of the high vacuum arc melting furnace is a predetermined value (for example, the pressure gauge in the furnace is 0.05 MPa). The melting temperature is set to melt only Ti in the raw material of the high entropy alloy to absorb the residual oxygen in the furnace chamber, so that there are no gas impurities in the furnace chamber that affect the melting, and then the temperature is increased to melt other components, thereby reducing the gas impurity elements and providing the purity of the high entropy alloy finally prepared.

[0030] In step S5, the current value is set to melt the raw materials in the furnace, for example, the current can be set to 400-600A; stirring is performed during the melting process so that materials of different elements can be evenly distributed, for example, electromagnetic stirring can be adopted.

[0031] In step S6, the alloy ingot is turned over, melted again, and cooled again to form an alloy ingot, and the above steps are repeated for a predetermined number of times. After the above-mentioned multiple turnings, melting and cooling, the elements inside the alloy are evenly distributed, and the completely molten alloy is cast and cooled into an alloy ingot. For example, a water-cooled copper mold can be used for casting. The following describes the preparation method of the high entropy alloy of the present application in detail through two embodiments. The expression of the high entropy alloy prepared in Example 1 is Ti 25 V 28 Zr 24 Nb 23 , the specific preparation steps are as follows:

[0032] High-purity Ti, high-purity V, high-purity Zr and high-purity Nb (for example, the purity of the above materials is ≥99.95%) are used as raw materials, and the oxide layer on the surface of the above raw materials is removed by sandpaper polishing, and then ultrasonic cleaning is performed with alcohol or acetone, and then blown dry after cleaning to obtain pure raw materials.

[0033] According to the expression Ti 25 V 28 Zr 24 Nb 23 Weigh the raw materials of each element according to the atomic ratio of the middle and lower subscripts, and the total mass of the raw materials weighed is (100±0.01) g.

[0034] Place weighed high-purity Ti, high-purity V, high-purity Zr and high-purity Nb into the crucible of a high vacuum arc melting furnace in order from low to high melting points, with Ti at the bottom, and close the furnace door.

[0035] The furnace chamber was evacuated to 5 Pa, and then high-purity argon gas with a purity of 99.999% was introduced, and then evacuated again. The above steps were repeated 3 times to complete the removal of gas impurities in the furnace chamber, and finally evacuated to 1×10 -3 Pa, high-purity argon is introduced as a protective gas until the surface pressure in the furnace reaches 0.05MPa.

[0036] The smelting furnace is powered on with a current of 400-600A. The smelting temperature is then set to only be able to melt Ti, which has the lowest melting point among the raw materials. After the titanium in the furnace cavity is melted, it can absorb the residual oxygen in the furnace cavity. Then the smelting temperature is increased to be able to melt Nb, which has the highest melting point among the raw materials, to achieve alloy smelting of all raw materials. At the same time, electromagnetic stirring is turned on. After each element raw material is completely melted for about 3 minutes, it is cooled to form an alloy ingot.

[0037] The alloy ingot is turned over and remelted, then turned over again and melted again, and repeated 5 times to make the elements inside the alloy evenly distributed. Finally, the completely molten alloy is poured into a water-cooled copper mold and quickly cooled into an ingot to obtain Ti 25 V 28 Zr 24 Nb 23 High entropy alloy.

[0038] The prepared Ti 25 V 28 Zr 24 Nb 23 The high entropy alloy is subjected to phase analysis before the hydrogen absorption test. An X-ray diffractometer (for example, RIGAKU D / MAX-RB) is used for phase analysis. The operating voltage for phase analysis is 40 kV, the operating current is 40 mA, the X-ray source is CuKα (λ=0.15406 nm), the scanning speed is 0.1 sec / step, and the scanning range is 10°-90°.

[0039] See also Figure 1 , Figure 1 The prepared Ti 25 V 28 Zr 24 Nb 23 X-ray diffraction (XRD) spectrum of high entropy alloy before hydrogen absorption test, curve 1 shows Ti 25 V 28 Zr 24 Nb 23 X-ray diffraction (XRD) spectrum of high entropy alloy before hydrogen absorption test, where the unit of the horizontal axis is angle. Figure 1 It can be seen from the XRD spectrum that curve 1 represents Ti 25 V 28 Zr 24 Nb 23 Before absorbing hydrogen, high entropy alloys present a single-phase BCC structure.

[0040] The prepared Ti 25 V 28 Zr 24 Nb 23 The high entropy alloy was tested for hydrogen storage performance. The cast high entropy alloy was tested using an MH-PCT-100 metal hydride hydrogen storage performance tester with a maximum test pressure of 9 MPa and a test accuracy of 0.0001 MPa. The high entropy alloy was divided into test samples of 3 mm × 3 mm × 3 mm blocks. Before the sample was tested, it was subjected to hydrogen absorption at room temperature and hydrogen release at 600 °C for activation treatment.

[0041] See also Figure 2 , Figure 2The Ti prepared in Example 1 is shown 25 V 28 Zr 24 Nb 23 Hydrogen absorption kinetic curve of high entropy alloy at 20℃ and 0.2MPa hydrogen pressure3.

[0042] The horizontal axis represents time and the vertical axis represents the amount of hydrogen absorption. It can be seen from the hydrogen absorption kinetic curve 3 that Ti 25 V 28 Zr 24 Nb 23 High entropy alloys have excellent hydrogen absorption kinetics at 20°C and 0.2MPa, with no obvious incubation period, and can reach a maximum hydrogen absorption capacity of 2.31wt.% in about 100s.

[0043] See also Figure 3 , Figure 3 Show Ti 25 V 28 Zr 24 Nb 23 The hydrogen absorption pressure-concentration-temperature (PCT) curve 4 of the high entropy alloy at 20°C, wherein the horizontal axis represents the hydrogen content and the vertical axis represents the equilibrium pressure. It can be seen from curve 4 that under 20°C conditions, as the equilibrium pressure increases, the maximum hydrogen absorption amount also increases, and can reach 2.28wt.% at 1MPa.

[0044] See also Figure 4 , Figure 4 The Ti prepared in Example 1 is shown 25 V 28 Zr 24 Nb 23 The hydrogen absorption kinetic curves of the high entropy alloy at 20°C and 0.2MPa hydrogen pressure for three cycles, curve 5 represents the first hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure, curve 6 represents the second hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure, and curve 7 represents the third hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure. It can be seen from curves 5, 6 and 7 that the Ti prepared in Example 1 25 V 28 Zr 24 Nb 23 The high entropy alloy repeatedly absorbed and desorbed hydrogen three times at 20°C and 0.2MPa, and the maximum hydrogen absorption amounts were approximately 2.31wt.%, 2.25wt.% and 2.22wt.%, respectively. It can be seen that after multiple cycles of hydrogen absorption and desorption, the hydrogen storage performance of the alloy did not decay significantly and remained above 96%.

[0045] The expression of the high entropy alloy prepared in Example 2 is Ti 24 V 26 Zr17 Nb 16 Hf 17 , the specific preparation steps are as follows:

[0046] Ti 24 V 26 Zr 17 Nb 16 Hf 17 The specific preparation steps of high entropy alloy are as follows:

[0047] High-purity Ti, high-purity V, high-purity Zr, high-purity Nb and high-purity Hf (for example, the purity of the above materials is ≥99.95%) are used as raw materials, the oxide layer on the surface of the above raw materials is removed by sandpaper polishing, and then ultrasonic cleaning is performed with alcohol or acetone, and then blown dry after cleaning to obtain pure raw materials.

[0048] According to the expression Ti 24 V 26 Zr 17 Nb 16 Hf 17 Weigh the raw materials of each element according to the atomic ratio of the middle and lower subscripts, and the total mass of the raw materials weighed is (100±0.01) g.

[0049] Put the weighed high-purity Ti, high-purity V, high-purity Zr, high-purity Nb and high-purity Hf into the crucible of the high vacuum arc melting furnace in order from low to high melting points, with Ti at the bottom, and close the furnace door.

[0050] The furnace chamber was evacuated to 5Pa, and then high-purity argon gas with a purity of 99.999% was introduced, and then vacuumed again. The above steps were repeated 3 times to complete the removal of gas impurities in the furnace chamber. Finally, the furnace chamber was evacuated to 1×10-3Pa, and high-purity argon gas was introduced as a protective gas until the surface pressure in the furnace reached 0.05MPa.

[0051] The smelting furnace is powered on with a current of 400-600A. The smelting temperature is then set to only be able to melt Ti, which has the lowest melting point among the raw materials. After the titanium in the furnace cavity is melted, it can absorb the residual oxygen in the furnace cavity. Then the temperature is raised to be able to melt Nb, which has the highest melting point among the raw materials, to achieve alloy smelting of all raw materials. At the same time, electromagnetic stirring is turned on. The raw materials of each element are completely melted for about 3 minutes and then cooled to form an alloy ingot.

[0052] The alloy ingot is turned over and remelted, then turned over again and melted again, and repeated 5 times to make the elements inside the alloy evenly distributed. Finally, the completely molten alloy is poured into a water-cooled copper mold and quickly cooled into an ingot to obtain Ti 24 V 26 Zr 17 Nb 16 Hf 17 High entropy alloy.

[0053] The prepared Ti 24 V 26 Zr 17 Nb 16 Hf 17 The high entropy alloy is subjected to phase analysis before the hydrogen absorption test. An X-ray diffractometer (for example, RIGAKU D / MAX-RB) is used for phase analysis. The operating voltage during phase analysis is 40 kV, the operating current is 40 mA, the X-ray source is CuKα (λ=0.15406 nm) rays, the scanning speed is 0.1 sec / step, and the scanning range is 10°-90°.

[0054] See also Figure 1 , Figure 1 The prepared Ti 24 V 26 Zr 17 Nb 16 Hf 17 X-ray diffraction (XRD) spectrum of high entropy alloy before hydrogen absorption test, curve 2 shows Ti 24 V 26 Zr 17 Nb 16 Hf 17 X-ray diffraction (XRD) pattern of high entropy alloy before hydrogen absorption test. Figure 1 It can be seen from the XRD spectrum that curve 2 represents Ti 24 V 26 Zr 17 Nb 16 Hf 17 Before absorbing hydrogen, high entropy alloys present a single-phase BCC structure.

[0055] The prepared Ti 24 V 26 Zr 17 Nb 16 Hf 17 The high entropy alloy was tested for hydrogen storage performance. The cast high entropy alloy was tested using an MH-PCT-100 metal hydride hydrogen storage performance tester with a maximum test pressure of 9 MPa and a test accuracy of 0.0001 MPa. The high entropy alloy was divided into test samples of 3 mm × 3 mm × 3 mm blocks. Before the sample was tested, it was subjected to hydrogen absorption at room temperature and hydrogen release at 600 °C for activation treatment.

[0056] See also Figure 5 , Figure 5 The Ti prepared in Example 2 is shown 24 V 26 Zr 17 Nb 16 Hf 17The hydrogen absorption kinetic curve 8 of high entropy alloy at 20°C and 0.2MPa hydrogen pressure. The horizontal axis represents time and the vertical axis represents the amount of hydrogen absorption. It can be seen from the hydrogen absorption kinetic curve 8 that Ti 24 V 26 Zr 17 Nb 16 Hf 17 High entropy alloys have excellent hydrogen absorption kinetics at 20°C and 0.2MPa, with no obvious incubation period, and can reach a maximum hydrogen absorption capacity of 1.57wt.% in about 75s.

[0057] See also Figure 6 , Figure 6 Show Ti 24 V 26 Zr 17 Nb 16 Hf 17 The hydrogen absorption pressure-concentration-temperature (PCT) curve 9 of the high entropy alloy at 20°C, wherein the horizontal axis represents the hydrogen content and the vertical axis represents the equilibrium pressure. It can be seen from curve 4 that at 20°C, as the equilibrium pressure increases, the maximum hydrogen absorption amount also increases, and can reach 1.63wt.% at 8MPa.

[0058] See also Figure 7 , Figure 7 The Ti prepared in Example 2 is shown 24 V 26 Zr 17 Nb 16 Hf 17 The hydrogen absorption kinetic curves of the high entropy alloy at 20°C and 0.2MPa hydrogen pressure for three cycles, curve 10 represents the first hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure, curve 11 represents the second hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure, and curve 12 represents the third hydrogen absorption kinetic curve at 20°C and 0.2MPa hydrogen pressure. It can be seen from curves 10, 11 and 12 that the alloy repeatedly absorbs and releases hydrogen three times at 20°C and 0.2MPa, and the maximum hydrogen absorption amounts are approximately 1.57wt.%, 1.50wt.% and 1.54wt.%, respectively. It can be seen that after multiple cycles of hydrogen absorption and desorption, the hydrogen storage performance of the alloy has no obvious attenuation and remains above 95%.

[0059] Regarding the embodiments of the present application, it should also be noted that, in the absence of conflict, the embodiments of the present application and the features therein can be combined with each other to obtain new embodiments.

[0060] The above are only specific implementation methods of the present application, but the protection scope of the present application is not limited thereto. The protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A high entropy alloy, characterized in that: The high entropy alloy comprises the following elements: Ti, V, Zr, Nb and Hf, Among them, the percentage of the atomic content of each element meets the following range: 23%≤Ti≤27%, 26%≤V≤30%, 17%≤Zr≤25%, 16%≤Nb≤22%, 0%≤Hf≤18%, and the sum of the atomic contents of the elements is 100%.

2. A method for preparing the high entropy alloy according to claim 1, characterized in that: The method comprises the following steps: S1: pretreating raw materials for preparing the high entropy alloy; S2: weighing the pretreated raw materials according to the proportions of the components of the high entropy alloy; S3: putting the weighed raw materials into a smelting device to be used for preparing the high entropy alloy; S4: treating the internal environment of the smelting equipment to remove oxygen; S5: melting and cooling the raw materials into alloy ingots in the smelting equipment; S6: Processing the alloy ingot to obtain a melt in which the elements constituting the high entropy alloy are evenly distributed, and casting the high entropy alloy after the alloy is completely melted.

3. The method according to claim 2, characterized in that In step S4, the smelting equipment is evacuated, and argon gas of a predetermined purity is introduced. The above operation is repeated a predetermined number of times until the vacuum degree reaches a predetermined value, and argon gas of a predetermined purity is introduced into the smelting equipment again so that the pressure of the smelting equipment is a predetermined value.

4. The method according to claim 2, characterized in that: In step S3, the weighed raw materials of each component are put into the smelting equipment in the order of melting point from low to high.

5. The method according to claim 4, characterized in that In step S4, the smelting temperature is set to melt only Ti in the raw material of the high entropy alloy, and after Ti is melted, the temperature is increased to melt other components.

6. The method according to claim 2, characterized in that In step S5, stirring is performed while melting.

7. The method according to claim 2, characterized in that In step S6, the alloy ingot is turned over, melted again, and cooled again to form an alloy ingot, and the above steps are repeated a predetermined number of times.

8. The method according to claim 2, characterized in that: In step S6, the completely molten alloy is cast into a water-cooled copper mold to obtain the high entropy alloy.

9. The method according to claim 2, characterized in that: In step S1, the raw material of the high entropy alloy is polished, cleaned and dried to remove impurities.

10. The method according to any one of claims 2 to 9, characterized in that: In step S5, the smelting current of the smelting equipment is 400-600A.

Citation Information

Cited By

  • TiCrNbV high-entropy hydrogen storage alloy with BCC structure and preparation method of TiCrNbV high-entropy hydrogen storage alloy

    CN120796812A