Preparation method and application of sodium vanadyl fluorophosphate single-crystal composite material

By performing alkali metal sodium doping and in-situ carbon coating in single crystal material of vanadyl phosphate, the problems of prone cracking and poor circulation stability of sodium ion battery cathode materials are solved, and the structural stability and electrical properties of the material are improved Chemical properties have promoted the commercial application of sodium ion batteries.

CN118910729APending Publication Date: 2024-11-08YUNNAN YUNTIANHUA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997614.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials are prone to cracking and have poor circulation stability, which limits the pace of their application.

Method used

The preparation method of sodium vanadyl fluorophosphate single crystal composite material is adopted, and the ion transport efficiency and structural stability of the material are improved through alkali metal sodium doping and in-situ carbon coating technology, reducing polarization voltage and volume changes, and enhancing the material's Rate performance and cycle life.

Benefits of technology

The high cycle stability and rate performance of sodium ion battery materials are achieved, which significantly improves the energy density and first-circle efficiency of the material, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910729A_ABST
    Figure CN118910729A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a sodium vanadyl fluorophosphate single crystal composite material, and relates to the technical field of sodium ion battery positive electrode materials. Comprising the following steps: stirring and dissolving a vanadium source and a carbon source in a solvent, then adding an alkali metal sodium site alkali metal doped element, a sodium source, a phosphorus source and a fluorine source, stirring and mixing uniformly, carrying out a hydrothermal reaction at 200-250 DEG C for 2-20 h, annealing the obtained alkali metal sodium site doped oxygen vanadium sodium fluorophosphate single crystal in an inert atmosphere at 350-800 DEG C for 0.1-5 h, and finally obtaining the alkali metal sodium site doped oxygen vanadium sodium fluorophosphate single crystal. The in-situ carbon-coated doped sodium vanadyl fluorophosphate single crystal composite material is obtained; the single crystallization of the prepared material can improve the structural stability of the material, and improve the rate capability and energy density of the material; the method has important significance in application of the material in a sodium ion battery with high energy density and long cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a preparation method and application of a sodium vanadium fluorophosphate single crystal composite material. Background Art

[0002] 2023 is considered the first year of commercial application of sodium-ion batteries. Due to its low cost, high safety, high power density and good electrochemical performance over a wide temperature range, sodium-ion batteries have attracted widespread attention in downstream low-speed electric vehicles, mining cars / heavy trucks, electric bicycles, low-speed electric ships and large-scale energy storage. Compared with lithium-ion batteries, the low energy density and short cycle life of sodium-ion batteries restrict the pace of their application. Therefore, it is urgent to develop a new type of sodium-ion battery electrode with high energy density and long cycle life.

[0003] The cathode material usually accounts for the highest part of the battery cost and largely determines the battery's sodium storage performance. It is currently the focus of research institutes and enterprises. Sodium vanadium fluorophosphate has a stable three-dimensional open framework structure that allows sodium ions to be reversibly embedded and de-embedded in three directions with little structural change, and has a high theoretical capacity (130mAhg -1 ) and high average operating voltage (~3.8V), making it a very promising cathode material for sodium-ion batteries.

[0004] However, the charge and discharge volume change of polycrystalline sodium vanadium fluorophosphate positive electrode materials usually leads to material cracking and poor cycle stability. Therefore, the single crystal structure of the material can effectively alleviate the volume change of the material, reduce the specific surface area of ​​the material and the growth of the surface SEI film. The long intracrystalline ion transmission distance of the single crystal material reduces the capacity and rate performance of the material. Therefore, the development of single crystal sodium vanadium fluorophosphate materials with fast ion transmission can accelerate the commercial application of this material. Summary of the invention

[0005] The invention provides a preparation method and application of a sodium vanadium oxyfluorophosphate single crystal composite material, which solves the problems of easy cracking and poor cycle stability of existing synthesized positive electrode materials during use.

[0006] To achieve the above purpose, the technical solution adopted by this application is:

[0007] A method for preparing a sodium vanadium fluorophosphate single crystal composite material comprises the following steps:

[0008] 1) taking a sodium source, a vanadium source, a phosphorus source and a fluorine source according to the element mass ratio Na:V:P:F=3:2:2:3, weighing an alkali metal doping element M, wherein the ratio of the alkali metal doping element M to the sodium element is 0.01-10%; weighing a reducing agent, wherein the reducing agent is a carbon source;

[0009] 2) adding the vanadium source and the carbon source into a beaker filled with pure water and stirring to form a solution; then adding the sodium source, the fluorine source and the phosphorus source into the above solution and continuing to stir and mix evenly, adjusting the pH of the solution to 4-9 with ammonia water to obtain a precursor solution; the amount of the carbon source is 120-180% of the amount required to reduce the pentavalent vanadium of the vanadium source to tetravalent vanadium;

[0010] 3) transferring the precursor solution obtained in 2) to a hydrothermal reactor, heating it to 200-250° C., reacting it at a constant temperature for 2-20 hours, then naturally cooling it to room temperature, and filtering to obtain a doped sodium vanadium fluorophosphate single crystal material;

[0011] 4) The sodium vanadium fluorophosphate single crystal material obtained in 3) is rapidly heated to 350-800° C. at a heating rate of 15-20° C. / min under an inert atmosphere, and then naturally cooled to room temperature after constant temperature reaction for 0.1-5 hours to obtain an amorphous carbon-coated sodium vanadium fluorophosphate doped single crystal composite material.

[0012] In order to prepare an in-situ carbon-coated alkali metal sodium-doped sodium vanadium fluorophosphate single crystal composite material, it is usually difficult to form point defects and impurity substitutions during the hydrothermal synthesis process. Therefore, the present method increases the hydrothermal temperature to above 200°C to improve the reactivity of the material so that the metal doping elements can form a stable substitution at the Na position, thereby avoiding the phenomenon that the doping elements inhibit the crystal growth of the material in the solid phase sintering method.

[0013] The addition of alkali metal ions can induce crystal orientation growth and shorten the transmission distance of sodium ions in the crystal. Alkali metal sodium doping can effectively improve the ion transmission efficiency of the material and reduce the polarization voltage during the charge and discharge process of the material. Carbon coating can effectively improve the surface electronic conductivity of the material, and improve the rate performance and first-cycle efficiency of the composite material while ensuring the high cycle stability of the material. In-situ carbon coating can effectively reduce the thickness and usage ratio of carbon coating, ensure the uniformity of amorphous carbon coating on the surface of material particles and the electronic conduction characteristics, improve the quality of active substances in the material and the energy density of the composite material. Single crystalization can effectively alleviate the uneven stress and particle breakage caused by volume change during the charge and discharge process of the material, and greatly improve the cycle life of the material. Through this strategy, the excellent characteristics of rapid electron ion conduction and greatly improved material structural stability are achieved, and a new high-performance micron-level single crystal composite material preparation process is obtained.

[0014] As a preferred technical solution, the vanadium source in 1) is one or more of vanadyl acetylacetonate, vanadium acetylacetonate, ammonium metavanadate, vanadium pentoxide and vanadyl sulfate;

[0015] The phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium phosphate and ammonium phosphate;

[0016] The sodium source is one or more of sodium fluoride, sodium chloride, sodium carbonate, sodium hydroxide, sodium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and sodium nitrate;

[0017] The fluoride source is one or more of sodium fluoride, ammonium fluoride, potassium fluoride and magnesium fluoride.

[0018] As a preferred technical solution, the vanadium source and carbon source in 2) are added to a beaker filled with pure water and stirred at a speed of 100 to 800 r / min for 0.1 to 2 h; in 2), the sodium source, fluorine source and phosphorus source are added to the above solution and stirred for 1 to 2 h to mix evenly.

[0019] As a preferred technical solution, the carbon source is glucose (C6H 12 O6), fructose (C6H 12 O6), sucrose (C 12 H 22 O 11 ), lactose (C 12 H 22 O 11 ) and maltose (β-C 12 H 22 O 11 ·H2O) or more.

[0020] As a preferred technical solution, the alkali metal doping element M described in 2) is one or more of lithium (Li), potassium (K), rubidium (Rb) and cesium (Cs).

[0021] As a preferred technical solution, the inert atmosphere in 4) is one or both of argon and nitrogen.

[0022] The invention also discloses a sodium vanadium oxyfluorophosphate single crystal composite material prepared by a method for preparing the sodium vanadium oxyfluorophosphate single crystal composite material.

[0023] The invention also discloses application of a sodium vanadium oxyfluorophosphate single crystal composite material in a sodium ion battery.

[0024] As a preferred technical solution, the positive electrode material of the sodium ion battery comprises the sodium vanadium fluorophosphate single crystal composite material.

[0025] The method adopts a sodium vanadium fluorophosphate single crystal composite material preparation method, which comprises the following steps: 1) taking a sodium source, a vanadium source, a phosphorus source and a fluorine source according to the element mass ratio Na:V:P:F=3:2:2:3, weighing an alkali metal doping element, wherein the ratio of the alkali metal doping element to the sodium element is 0.01-10%; weighing a reducing agent, wherein the reducing agent is a carbon source; 2) adding the vanadium source and the carbon source into a beaker filled with pure water and stirring to form a solution; then adding the sodium source, the fluorine source and the phosphorus source into the above solution, continuing to stir and mix uniformly, and adjusting the pH value of the solution to between 4 and 9 by using ammonia water to obtain the above-mentioned composite material. The method comprises the following steps: a) transferring the precursor solution obtained in 2) to a hydrothermal reactor, heating the precursor solution to 200-250°C, keeping the temperature constant for 2-20 hours, and then naturally cooling the precursor solution to room temperature. After filtration, the doped sodium vanadium oxyfluorophosphate single crystal material is obtained. 4) heating the sodium vanadium oxyfluorophosphate single crystal material obtained in 3) to 350-800°C at a heating rate of 20°C / min under an inert atmosphere, keeping the temperature constant for 0.1-5 hours, and then naturally cooling the precursor solution to room temperature to obtain an amorphous carbon-coated sodium vanadium oxyfluorophosphate single crystal composite material.

[0026] The present invention has the following beneficial effects:

[0027] (1) The present invention adopts alkali metal sodium doping and in-situ carbon coating composite modification technology. Sodium doping can expand the sodium site space, which will effectively improve the transmission efficiency of sodium ions during the charge and discharge process of the material, reduce the polarization voltage of the material, and improve the first cycle efficiency and rate performance of the material;

[0028] (2) Alkali metal sodium doping can change the growth direction of the crystal during the reaction process, inducing rapid oriented growth of the crystal salt in the Z direction, which is beneficial to the rapid transmission of sodium ions in the x and y directions, reducing battery polarization and improving the capacity and rate performance of the material;

[0029] (3) At the same time, optimizing the alkali metal sodium doping content and type can improve the structural stability of the material, reduce the volume change of the material during charging and discharging, and alleviate the problem of grain breakage and shedding caused by volume change, and rapid battery capacity decay;

[0030] (4) In-situ carbon coating can effectively reduce the thickness of the carbon coating, improve the utilization efficiency of carbon materials and the electronic conductivity of the material particle surface, increase the proportion of active substances in the material, reduce battery polarization and improve the material capacity, first cycle efficiency and rate performance.

[0031] (5) The present invention prepares an in-situ carbon-coated alkali metal sodium-doped sodium vanadyl fluorophosphate single crystal composite material, which is consistent with the tetragonal crystal structure of sodium vanadyl fluorophosphate by X-ray diffraction testing, and the X-ray photoelectron spectroscopy also shows that amorphous carbon is successfully coated and sodium-position alkali metal elements are successfully doped. Scanning electron microscope photos show the columnar structure of the material, and its accessory energy spectrometer test shows that all elements are evenly distributed. The electrochemical performance test results show that the first-cycle efficiency of the doped single crystal composite material is significantly improved, the capacity rate performance is significantly enhanced, and the high cycle stability of the single crystal material is maintained.

[0032] (6) In-situ carbon-coated alkali metal sodium-doped sodium vanadium fluorophosphate single crystal composite material. Alkali metal sodium doping will effectively improve the sodium ion transmission efficiency and structural stability during the charge and discharge process of the material, reduce the volume change of the material, and in-situ carbon coating can effectively reduce the thickness and usage ratio of the carbon coating, ensure the uniformity of amorphous carbon coating on the surface of the material particles and the electronic conduction characteristics, and improve the quality of the active substances in the material and the energy density of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a microscopic SEM image of the comparative example sample of the present invention;

[0034] Figure 2 This is a microscopic SEM image of the sample of Example 1 of the present invention;

[0035] Figure 3 This is a microscopic SEM image of the sample of Example 2 of the present invention;

[0036] Figure 4 This is a microscopic SEM image of the sample of Example 3 of the present invention;

[0037] Figure 5 This is a microscopic SEM image of the sample of Example 4 of the present invention;

[0038] Figure 6 This is a microscopic SEM image of the sample of Example 5 of the present invention;

[0039] Figure 7 XRD patterns of samples of comparative example and examples 1 to 5 of the present invention;

[0040] Figure 8 The SEM and EDS images of the sample of Example 2 of the present invention;

[0041] Fig. 9 This is a high-magnification TEM image of the sample in Example 2 of the present invention;

[0042] Fig.10 This is the electron diffraction pattern of the sample of Example 2 of the present invention;

[0043] Fig.11The cycle curves of Example 2 of the present invention and the comparative example samples at 0.2C and 1C rates;

[0044] Fig.12 This is a cycle curve diagram of Example 2 of the present invention at a 10C rate. DETAILED DESCRIPTION

[0045] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0046] Embodiment 1:

[0047] 1) according to the element mass ratio Na:V:P:F=3:2:2:3, take a certain amount of sodium fluoride, ammonium metavanadate and ammonium dihydrogen phosphate, 10% molar vanadium of sucrose, and 0.1% molar sodium of lithium fluoride;

[0048] 2) adding the ammonium metavanadate and sucrose in 1) into a beaker filled with ultrapure water whose volume is 60% of the volume of the hydrothermal kettle and stirring to form a solution at a stirring speed of 600 r / min for 0.1 h; adding sodium fluoride, lithium fluoride and ammonium dihydrogen phosphate into the solution and continuing stirring for 2 h, adjusting the pH of the precursor solution to 7 by dropping ammonia water to obtain a uniformly mixed precursor solution;

[0049] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 200° C., keeping the temperature constant for 20 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0050] 4) The sodium vanadium fluorophosphate single crystal material in step 3) is heated to 500° C. at a heating rate of 20° C. / min under an argon atmosphere, kept at this temperature for 2 hours, and then naturally cooled to room temperature to obtain an in-situ carbon-coated lithium-doped sodium vanadium fluorophosphate single crystal composite material (Na 3-x Li x V2O2(PO4)2F / C).

[0051] Embodiment 2:

[0052] 1) according to the element mass ratio Na:V:P:F=3:2:2:3, take a certain amount of sodium fluoride, ammonium metavanadate and sodium dihydrogen phosphate, 30% of the molar number of vanadium element glucose, and 10% of the molar number of sodium element potassium fluoride;

[0053] 2) adding the ammonium metavanadate and glucose in step 1) into a beaker of ultrapure water and stirring to form a solution at a stirring speed of 500 r / min for 2 h; adding sodium fluoride, potassium fluoride and sodium dihydrogen phosphate to the solution and continuing stirring for 2 h, adjusting the pH of the precursor solution to 7 by dropping ammonia water to obtain a uniformly mixed precursor solution;

[0054] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 250° C., keeping the temperature constant for 2 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0055] 4) The sodium vanadium fluorophosphate single crystal material in step 3) is heated to 300° C. at a heating rate of 15° C. / min under an argon atmosphere, kept at this temperature for 5 hours, and then naturally cooled to room temperature to obtain an in-situ carbon-coated potassium-doped sodium vanadium fluorophosphate single crystal composite material (Na 3-x K x V2O2(PO4)2F / C).

[0056] Embodiment 3:

[0057] 1) according to the element mass ratio Na:V:P:F=3:2:2:3, a certain amount of sodium fluoride, vanadium acetylacetonate and sodium phosphate, 12% molar amount of lactose of vanadium element and 12% molar amount of glucose of vanadium element, and 2% molar amount of potassium carbonate of sodium element are taken;

[0058] 2) adding the vanadium acetylacetonate, glucose and lactose in step 1) into a beaker of ultrapure water and stirring to form a solution at a stirring speed of 400 r / min for 0.5 h; adding sodium fluoride, potassium carbonate and sodium phosphate to the solution and continuing stirring for 2 h, adjusting the pH of the precursor solution to 7 by dropping ammonia water to obtain a uniformly mixed precursor solution;

[0059] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 220° C., keeping the temperature constant for 10 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0060] 4) The sodium vanadium fluorophosphate single crystal material in step 3) is heated to 800° C. at a heating rate of 20° C. / min under an argon atmosphere, kept at this temperature for 0.1 h, and then naturally cooled to room temperature to obtain an in-situ carbon-coated sodium vanadium fluorophosphate single crystal composite material (Na 3-y K y V2O2(PO4)2F / C).

[0061] Embodiment 4:

[0062] 1) according to the element mass ratio Na:V:P:F=3:2:2:3, a certain amount of sodium fluoride, vanadium pentoxide and ammonium dihydrogen phosphate, 7.5% vanadium element molar number of maltose and 7.5% vanadium element molar number of sucrose, and 2% molar number of sodium element potassium hydroxide are taken;

[0063] 2) adding vanadium pentoxide, maltose and sucrose in step 1) into a beaker of ultrapure water and stirring to form a solution at a stirring speed of 600 r / min for 1 h; adding sodium fluoride, potassium carbonate and ammonium dihydrogen phosphate to the solution and continuing stirring for 2 h, and adjusting the pH of the precursor solution to 9 by dropping ammonia water to obtain a uniformly mixed precursor solution;

[0064] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 220° C., keeping the temperature constant for 5 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0065] 4) The sodium vanadium fluorophosphate single crystal material in step 3) is heated to 600° C. at a heating rate of 20° C. / min under an argon atmosphere, kept at this temperature for 1 hour, and then naturally cooled to room temperature to obtain an in-situ carbon-coated sodium vanadium fluorophosphate single crystal composite material (Na 3- z K z V2O2(PO4)2F / C).

[0066] Embodiment 5:

[0067] 1) taking a certain amount of sodium fluoride, sodium sulfate, vanadium pentoxide and phosphoric acid, an appropriate amount of glucose, and cesium fluoride accounting for 1% molar number of the sodium element according to the element mass ratio Na:V:P:F=3:2:2:3;

[0068] 2) adding ammonium metavanadate and glucose in step 1) into a beaker of ultrapure water and stirring to form a solution at a stirring speed of 600 r / min for 1 h; adding sodium fluoride, sodium sulfate, cesium fluoride and diammonium phosphate to the solution and continuing stirring for 2 h, adjusting the pH of the precursor solution to 4 by dropping ammonia water to obtain a uniformly mixed precursor solution;

[0069] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 250° C., keeping the temperature constant for 16 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0070] 4) The sodium vanadium fluorophosphate single crystal material in step 3) is heated to 350° C. at a heating rate of 20° C. / min under an argon atmosphere, kept at this temperature for 2 hours, and then naturally cooled to room temperature to obtain an in-situ carbon-coated sodium vanadium fluorophosphate single crystal composite material (Na 3- x Cs x V2O2(PO4)2F / C).

[0071] Comparative Example:

[0072] 1) According to the element mass ratio Na:V:P:F=3:2:2:3, take a certain amount of sodium fluoride, ammonium metavanadate and ammonium dihydrogen phosphate, and take an appropriate amount of oxalic acid dihydrate;

[0073] 2) Add the ammonium metavanadate and oxalic acid dihydrate in step 1) into a beaker of ultrapure water to form a solution, and heat the solution and stir until the solution changes color to light green. Add sodium fluoride and ammonium dihydrogen phosphate to the solution and continue stirring for 2 hours to obtain a uniformly mixed precursor solution;

[0074] 3) transferring the precursor solution in step 2) to a hydrothermal reactor, heating it to 190° C., keeping the temperature constant for 16 hours, and then naturally cooling it to room temperature. After filtering, a sodium vanadium fluorophosphate single crystal material can be obtained;

[0075] 4) The sodium vanadium oxyfluorophosphate single crystal material in step 3) is heated to 700° C. at a heating rate of 1° C. / min under an argon atmosphere, kept at this temperature for 0.5 h, and then naturally cooled to room temperature to obtain a sodium vanadium oxyfluorophosphate single crystal material (Na3V2O2(PO4)2F).

[0076] A series of physical properties of the in-situ carbon-coated alkali metal sodium-doped sodium vanadium fluorophosphate composite materials prepared in Examples 1 to 5 and the comparative example were characterized, and the results are shown in the figure. Figure 1 to Figure 6 The SEM images of the in-situ carbon-coated alkali metal sodium-doped sodium vanadium fluorophosphate single crystal composite materials obtained in the comparative example and Examples 1 to 5 illustrate that the prepared sodium vanadium fluorophosphate has a micron-scale tetragonal columnar morphology. Figure 7 The XRD diagram of the in-situ carbon-coated alkali metal sodium doped sodium vanadium fluorophosphate single crystal composite material obtained in the comparative example and Examples 1 to 5 shows that the obtained composite materials are all tetragonal I4 / mmm type point group structures, which are consistent with the literature. It can be clearly seen from the figure that with the addition of alkali metal elements, the peak intensity of the (002) crystal plane in the z direction of the material is significantly enhanced and becomes the strongest peak, indicating that the addition of alkali metal elements can induce the growth of the material in the z direction. At the same time, the x and y directions are the fastest directions for sodium ion transmission. Rapid growth in the z direction can reduce the size in the xy direction, which is conducive to the rapid transmission of sodium ions in the single crystal structure. Figure 8 The SEM and element distribution diagram of the in-situ carbon-coated potassium-doped sodium vanadium fluorophosphate single crystal composite material obtained in Example 2 indicate that amorphous carbon is uniformly coated on the surface of the material, and Na, V, P, F and the doping element K are uniformly distributed on the single crystal particles. Fig. 9 and 10 The high-resolution TEM and transmission electron diffraction patterns of the in-situ carbon-coated potassium-doped sodium vanadium fluorophosphate single crystal composite material obtained in Example 2, the uniform and single sodium vanadium fluorophosphate (202) crystal plane lattice fringes in the TEM image, and the obvious single crystal diffraction pattern indicate that the prepared material is a single crystal particle.

[0077] Example 1 and the comparative example were used as the positive electrode, the metal sodium sheet was used as the negative electrode, the glass fiber membrane was used as the separator, the solute was 1M NaClO4, the solvent was a mixture of EC (ethylene carbonate) and DEC (diethyl carbonate) (volume ratio 1:1), the additive was 5% FEC as the electrolyte, and the aluminum foil was used as the current collector to assemble a CR2016 button-type sodium ion battery for electrochemical performance testing. The results are shown in Fig.11 As shown, the in-situ carbon-coated potassium-doped sodium vanadium fluorophosphate single crystal composite material sample obtained in Example 2 and the comparative example were subjected to constant current charge and discharge tests at a current density of 0.2C. Compared with the comparative example, the specific capacity and cycle stability of the doped sample were significantly improved.

[0078] Among them, the discharge specific capacities of Example 2 and the comparative example at 0.2C and 1C rates are 125.0 and 119.1 mAh / g, respectively, which are significantly higher than 124.2 and 118.2 mAh / g of the comparative example. After 150 cycles at 1C rate, the specific capacities of Example 2 and the comparative example are maintained at 115.5 mAh / g and 113.4 mAh / g, respectively, with retention rates of 97.9% and 96%, respectively, indicating that the in-situ carbon-coated potassium-doped sodium vanadium fluorophosphate single crystal composite material has better capacity, rate and cycle performance. Fig.12 The cycling performance of Example 2 at a 10C rate is demonstrated, wherein the efficiency of the composite material of Example 2 during charge and discharge is as high as 99.9%, indicating that it has good structural stability, and the 10C rate capacity reaches 75.0 mAh / g, and after 2500 cycles it still maintains 70.8 mAh / g, with a retention rate of 94.3%, indicating its good rate characteristics and ultra-high cycle stability.

[0079] Aiming at the characteristics of low energy density, poor rate performance and unsatisfactory cycle performance of sodium vanadium fluorophosphate, the present invention adopts a strategy of combining in-situ carbon coating and alkali metal sodium doping. The addition of alkali metal ions can induce crystal orientation growth and shorten the transmission distance of sodium ions in the crystal. The alkali metal sodium doping strategy can improve the structural stability of the single crystal structure and the sodium ion transmission efficiency. The in-situ carbon coating strategy can improve the coating uniformity of the carbon material and reduce the amount of carbon material, thereby ensuring good electronic conduction characteristics on the surface of the material, improving the energy density and capacity rate performance of the material, and having important significance for expanding the application field of the material in sodium ion batteries.

[0080] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a sodium vanadium fluorophosphate single crystal composite material, characterized in that: The following steps are involved: 1) according to the element ratio Na:V:P:F=3:2:2:3, a sodium source, a vanadium source, a phosphorus source and a fluorine source are taken, and an alkali metal doping element M is weighed, wherein the ratio of the alkali metal doping element M to the sodium element is 0.01-10%; a reducing agent is weighed, wherein the reducing agent is a carbon source; 2) adding the vanadium source and the carbon source into a beaker filled with ultrapure water and stirring to form a solution; then adding the sodium source, the fluorine source and the phosphorus source into the above solution and continuing to stir and mix evenly, adjusting the pH of the solution to 4-9 with ammonia water to obtain a precursor solution; the content of the carbon source is 120-180% of the amount required to reduce the pentavalent vanadium of the vanadium source to tetravalent vanadium; 3) transferring the precursor solution obtained in 2) to a hydrothermal reactor, heating it to 200-250° C., reacting it at a constant temperature for 2-20 hours, then naturally cooling it to room temperature, and filtering to obtain a doped sodium vanadium fluorophosphate single crystal material; 4) The sodium vanadium fluorophosphate single crystal material obtained in 3) is rapidly heated to 350-800° C. at a heating rate of 15-20° C. / min under an inert atmosphere, and then naturally cooled to room temperature after constant temperature reaction for 0.1-5 hours to obtain an amorphous carbon-coated sodium vanadium fluorophosphate doped single crystal composite material.

2. The method for preparing a sodium vanadium fluorophosphate single crystal composite material according to claim 1, characterized in that: The vanadium source in 1) is one or more of vanadyl acetylacetonate, vanadium acetylacetonate, ammonium metavanadate, vanadium pentoxide and vanadyl sulfate; The phosphorus source is one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium phosphate and ammonium phosphate; The sodium source is one or more of sodium fluoride, sodium chloride, sodium carbonate, sodium hydroxide, sodium sulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate and sodium nitrate; The fluoride source is one or more of sodium fluoride, ammonium fluoride, potassium fluoride and magnesium fluoride.

3. The method for preparing a sodium vanadium fluorophosphate single crystal composite material according to claim 1, characterized in that: The vanadium source and carbon source in 2) are added to a beaker filled with pure water, and the stirring speed is 100-800 r / min for 0.1-2 h; the sodium source, fluorine source and phosphorus source in 2) are then added to the above solution and stirred for 1-2 h to mix evenly.

4. The method for preparing a sodium vanadium fluorophosphate single crystal composite material according to claim 1, characterized in that: The carbon source is one or more of glucose, fructose, sucrose, lactose and maltose.

5. The method for preparing a sodium vanadyl fluorophosphate single crystal composite material according to claim 1, characterized in that: The alkali metal doping element M described in 2) is one or more of lithium, potassium, rubidium and cesium.

6. A method for preparing a sodium vanadyl fluorophosphate single crystal composite material according to claim 1, characterized in that: The inert atmosphere in 4) is one or both of argon and nitrogen.

7. A sodium vanadyl fluorophosphate single crystal composite material prepared by the method for preparing a sodium vanadyl fluorophosphate single crystal composite material according to any one of claims 1 to 6.

8. Use of the sodium vanadyl fluorophosphate single crystal composite material as claimed in claim 7 in a sodium ion battery.

9. Use of a sodium vanadyl fluorophosphate single crystal composite material in a sodium ion battery as claimed in claim 8, characterized in that: The positive electrode material of the sodium ion battery comprises the sodium vanadium fluorophosphate single crystal composite material.