Preparation method for improving magnetic performance of cerium-rich rare earth permanent magnet

By adding Gd to the cerium-rich rare earth permanent magnet raw material and adopting a specific process flow, the problem of low magnetic performance under high Ce content is solved, the coercivity and stability of the magnet are significantly improved, and the high-performance cerium-rich rare earth permanent Magnet preparation.

CN118919275APending Publication Date: 2024-11-08NINGBO NEWLAND MAGNET IND CORP LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411144811.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult to obtain excellent comprehensive magnetic properties when cerium-rich rare earth permanent magnets have high Ce content, and their chemical composition is complex and sensitive to the preparation process, which can easily lead to performance downshift or product scrapping.

Method used

A specific proportion of Gd is added to the raw materials, and cerium-rich rare earth permanent magnets are prepared through quick-condensation, hydrogen breaking, airflow grinding, magnetic field orientation molding, vacuum sintering and two-stage tempering processes, and the tempering temperature difference and process parameters are adjusted to improve magnetic performance. .

Benefits of technology

It significantly improves the coercive force, residual magnetism, magnetic energy product and squareness of the magnet, improves the stability and comprehensive performance of magnetic properties, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001921360000041
    Figure BDA0005001921360000041
Patent Text Reader

Abstract

The preparation method for improving the magnetic performance of the cerium-rich rare earth permanent magnet is characterized by comprising the following steps that S1, raw materials of the cerium-rich rare earth permanent magnet are provided; s2, rapid hardening; s3, powder preparation; s4, forming is conducted; and S5, sintering. Wherein the first-stage tempering temperature is lower than the second-stage tempering temperature, and the difference between the first-stage tempering temperature and the second-stage tempering temperature is 120-280 DEG C. According to the preparation method for improving the magnetic performance of the cerium-rich rare earth permanent magnet, the coercive force of the magnet can be obviously improved by adding a certain proportion of Gd into the raw materials under the conditions that the cerium content is the same and the total amount of rare earth is the same, the residual magnetism is equivalent to that of a method without adding Gd, and the squareness is higher than that of a method without adding Gd. Relatively high comprehensive magnetic performance is realized; under the condition that the chemical components are completely the same, compared with a traditional process, the residual magnetism is obviously improved by changing the tempering process, the differences of the residual magnetism, the coercive force, the magnetic energy product and the squareness among the heats are small, and the magnetic performance stability is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method for improving the magnetic properties of a cerium-rich rare earth permanent magnet. Background Art

[0002] R-Fe-B rare earth permanent magnet materials have excellent magnetic properties and are widely used in products such as electric vehicles, wind power generation, electric bicycles, robots, as well as audio equipment, communication products, medical equipment, home appliances, magnetic separation equipment and other fields. They have become irreplaceable materials and play an important role in the field of high-tech in today's society.

[0003] The main preparation processes of R-Fe-B rare earth permanent magnets include sintering, bonding, hot pressing / hot deformation, etc. Among them, sintered rare earth iron boron magnets have the highest comprehensive magnetic properties. In order to save the use of scarce rare earths, balance the use of rare earths, and reduce production costs, in recent years, the use of high-abundance rare earth metals such as La, Ce, and Y in R-Fe-B magnets has continued to increase, among which cerium-rich rare earth permanent magnets have been widely recognized. However, the current problems are as follows: 1. Due to the Ce2Fe 14 The magnetocrystalline anisotropy field and saturation magnetization of phase B are significantly lower than those of (Nd,Pr)2Fe 14 B. When the Ce content is high, it is difficult for cerium-rich rare earth magnets to obtain excellent comprehensive magnetic properties; 2. The chemical composition of cerium-rich rare earth magnets is complex, and the microstructure is sensitive to the preparation process, especially the heat treatment temperature. In the case of inappropriate preparation process, it is easy to cause product performance downgrade or even product scrapping, causing serious losses. Therefore, it is necessary to optimize the chemical composition and preparation process of cerium-rich magnets to improve magnetic properties and enhance their stability. Summary of the invention

[0004] The invention provides a preparation method for improving the magnetic properties of a cerium-rich rare earth permanent magnet.

[0005] The technical solution adopted by the present invention to solve the above technical problems is:

[0006] A preparation method for improving the magnetic properties of cerium-rich rare earth permanent magnets, characterized in that it comprises the following steps:

[0007] S1, providing the raw material of the cerium-rich rare earth permanent magnet, the cerium-rich magnet composition is Ce x G y R z Fe 100-x-y-z-b-c M a B b, wherein R is at least one of Nd, Pr, Dy, Tb, and Ho, M is at least one of Co, Al, Cu, Ga, Nb, Zr, and Ti, 6≤x≤16, 0.5≤y≤2, 10≤z≤28, 0.1≤a≤5, 0.85≤c≤0.94, 29≤x+y+x≤33; and 5≤x / y≤10;

[0008] S2, rapid setting: using rapid setting process to prepare cerium-rich rare earth iron boron alloy rapid setting sheet;

[0009] S3, powder making: crushing the cerium-rich rare earth iron boron alloy quick-setting flakes into fine powder by hydrogen crushing and air flow milling process;

[0010] S4, forming: the fine powder after air jet milling is subjected to magnetic field orientation forming and isostatic pressing process to prepare cerium-rich rare earth iron boron alloy green body;

[0011] S5, sintering: preparing the formed green body into the cerium-rich rare earth permanent magnet through vacuum sintering and tempering process, using a two-stage tempering process; wherein the first-stage tempering temperature is lower than the second-stage tempering temperature, and the two tempering temperatures differ by 120-280°C.

[0012] Preferably, in step S1, 6≤x / y≤8.

[0013] Preferably, in step S2, the maximum melting temperature is 1450-1480°C.

[0014] Preferably, in step S3, the average particle size of the fine powder is 2.6-3.2 um.

[0015] Preferably, in step S4, the intensity of the molding magnetic field is 1.5-2.0 T, the oxygen content of the molding press is less than or equal to 300 ppm, and the isostatic pressing pressure is 180-220 MPa.

[0016] Preferably, in step S5, during the heating process, when the temperature is at 100-150°C, it is kept warm for 0.5-1 hour; during the sintering process, the sintering temperature is 1020-1080°C, the vacuum degree is less than 0.1 Pa, and the time is 4-10 hours.

[0017] Preferably, in step S5, during the sintering process, the primary tempering temperature is 420-500° C., the tempering time is 2-6 hours, and the secondary tempering temperature is 600-700° C., the tempering time is 2-6 hours.

[0018] Preferably, in step S5, the primary tempering temperature and the secondary tempering temperature differ by 150-200°C.

[0019] Preferably, in step S1, the raw material of the cerium-rich rare earth permanent magnet, in terms of the mass percentage of each component element, has the following specific components: Ce7Gd1Nd16.7 Pr 5.5 Al 0.1 Cu 0.15 Zr 0.25 Fe 68.38 B 0.92 , where the ratio of Ce to Gd content is 7.

[0020] Preferably, in step S1, the raw material of the cerium-rich rare earth permanent magnet, calculated by mass percentage of each component element, has the following specific components: Ce 10 G 1.6 Nd 15.1 Pr 4.8 Al 0.3 Cu 0.2 Zr 0.3 Ti 0.2 Ga 0.15 Fe 66.45 B 0.9 , where the ratio of Ce to Gd content is 6.25.

[0021] Compared with the prior art, the preparation method of the present invention improves the magnetic properties of cerium-rich rare earth permanent magnets. By adding a certain proportion of Gd to the raw materials under the condition of the same cerium content and the same total amount of rare earth, the coercive force of the magnet can be significantly improved, the remanence is equivalent to that of the method without adding Gd, and the squareness is higher than that of the method without adding Gd, and the magnet has higher comprehensive magnetic properties. By changing the tempering process, the remanence is significantly improved compared with the traditional process under the condition of completely the same chemical composition, and the differences in remanence, coercive force, magnetic energy product and squareness between furnaces are small, and the magnetic property stability is high. DETAILED DESCRIPTION

[0022] The present invention is described in further detail below.

[0023] A preparation method for improving the magnetic properties of cerium-rich rare earth permanent magnets comprises the following steps:

[0024] Embodiment 1:

[0025] S1, providing raw materials of cerium-rich rare earth permanent magnets, wherein the cerium-rich magnet composition is Ce by mass percentage. x G y R z Fe 100-x-y-z-b-c M a B b; Wherein, R is at least one of Nd, Pr, Dy, Tb, and Ho, M is at least one of Co, Al, Cu, Ga, Nb, Zr, and Ti, 6≤x≤16, 0.5≤y≤2, 10≤z≤28, 0.1≤a≤5, 0.85≤c≤0.94, 29≤x+y+x≤33, and 5≤x / y≤10, preferably 6≤x / y≤8.

[0026] Among them, according to the mass percentage of each component element, the specific composition of the raw material is: Ce7Gd1Nd 16.7 Pr 5.5 Al 0.1 Cu 0.15 Zr 0.25 Fe 68.38 B 0.92 , where the ratio of Ce to Gd content is 7;

[0027] S2, rapid setting: using rapid setting process to prepare cerium-rich rare earth iron boron alloy rapid setting sheet;

[0028] The maximum melting temperature during the rapid solidification process is 1450-1480°C, preferably, the maximum melting temperature is 1480°C;

[0029] S3, powder making: using hydrogen crushing and air flow milling process to crush the cerium-rich rare earth iron boron alloy quick-setting flakes into fine powder;

[0030] The average particle size of the fine powder is 2.6-3.2um, preferably 3.0um;

[0031] S4, forming: the fine powder after air jet milling is subjected to magnetic field orientation forming and isostatic pressing process to prepare cerium-rich rare earth iron boron alloy green body;

[0032] The intensity of the forming magnetic field is 1.5-2.0T, preferably 1.8T, the oxygen content of the forming press is less than or equal to 300ppm, and the isostatic pressing pressure is 180-220MPa, preferably 200MPa;

[0033] S5, sintering: preparing the formed green body into the cerium-rich rare earth permanent magnet through vacuum sintering and tempering process, using a two-stage tempering process; the first-stage tempering temperature is lower than the second-stage tempering temperature, and the difference between the two tempering temperatures is 120-280°C;

[0034] In the heating exhaust and dehumidification stage, during the heating process, when the temperature is between 100 and 150°C, the temperature is kept at 0.5 to 1 hour, the sintering temperature is 1020 to 1080°C, the vacuum degree is less than 0.1 Pa, and the time is 4 to 10 hours; preferably, during the heating process, when the temperature is 120°C, the temperature is kept at 1 hour; and the sintering temperature is 1070°C, the vacuum degree is 3×10 -2 , the heat preservation time is 5 hours;

[0035] During the sintering process, the primary tempering temperature is 420-500°C, the tempering time is 2-6 hours, the secondary tempering temperature is 600-700°C, and the tempering time is 2-6 hours; preferably, the primary tempering temperature is 450°C, the holding time is 3 hours, the secondary tempering temperature is 620°C, and the holding time is 5 hours.

[0036] The performance test of the prepared cerium-rich magnet was conducted using a permanent magnet performance measuring instrument at room temperature. The same process was used to produce three batches of products, and the magnetic properties of 5 samples were randomly tested in each batch. The test results are shown in Table 1:

[0037] Table 1 Magnetic properties test results of the magnets prepared in Example 1

[0038]

[0039]

[0040] Comparative Example 1

[0041] The cerium-rich magnet was prepared by the same process as in Example 1, except that the chemical composition used in Control Example 1 was Ce7Nd 17.4 Pr 5.8 Al 0.15 Cu 0.15 Zr 0.25 Fe 68.33 B 0.92 The raw material of comparative example 1 does not contain Gd. The same process is adopted to produce three furnaces of products. The test method is the same as that of embodiment 1. The test results are shown in Table 2:

[0042] Table 2 Magnetic properties test results of the magnets prepared in Comparative Example 1

[0043] Test heat Remanence(kGs) Coercivity(kOe) Magnetic energy product (MGOe) Squareness(%) 1# 13.51-13.62 12.1-12.6 43.2-44.4 95.2-96.7 2# 13.45-13.61 11.8-12.5 43.7-44.6 95.8-96.2 3# 13.50-13.63 11.6-12.3 43.6-44.7 95.5-97.4

[0044] It can be seen from the above-mentioned Example 1 and Control Example 1 that, when the cerium content and the total amount of rare earth are the same, adding a certain proportion of Gd to the raw material can significantly improve the coercive force of the magnet, the remanence is equivalent to that of Control Example 1, the squareness is higher than that of Control Example 1, and it has higher comprehensive magnetic properties.

[0045] Embodiment 2:

[0046] S1, providing raw materials of cerium-rich rare earth permanent magnets, wherein the cerium-rich magnet composition is Ce by mass percentage. x G y R z Fe 100-x-y-z-b-c M a B b; Wherein, R is at least one of Nd, Pr, Dy, Tb, and Ho, M is at least one of Co, Al, Cu, Ga, Nb, Zr, and Ti, 6≤x≤16, 0.5≤y≤2, 10≤z≤28, 0.1≤a≤5, 0.85≤c≤0.94, 29≤x+y+x≤33, and 5≤x / y≤10, preferably, 6≤x / y≤8;

[0047] Among them, according to the mass percentage of each component element, the specific composition of the raw material is: Ce 10 G 1.6 Nd 15.1 Pr 4.8 Al 0. 3Cu 0.2 Zr 0.3 Ti 0.2 Ga 0.15 Fe 66.45 B 0.9 , where the ratio of Ce to Gd content is 6.25;

[0048] S2, rapid setting: using rapid setting process to prepare cerium-rich rare earth iron boron alloy rapid setting sheet;

[0049] The highest melting temperature during the rapid solidification process is 1450-1480°C, preferably, the highest melting temperature is 1480°C.

[0050] S3, powder making: using hydrogen crushing and air flow milling process to crush the cerium-rich rare earth iron boron alloy quick-setting flakes into fine powder;

[0051] The average particle size of the fine powder is 2.6-3.2um, preferably 2.8um;

[0052] S4, forming: the fine powder after air jet milling is subjected to magnetic field orientation forming and isostatic pressing process to prepare cerium-rich rare earth iron boron alloy green body;

[0053] The strength of the forming magnetic field is 1.5-2.0T, the oxygen content of the forming press is less than or equal to 300ppm, and the isostatic pressing pressure is 180-220MPa, wherein the strength of the forming magnetic field is preferably 1.8T, and the isostatic pressing pressure is preferably 200MPa;

[0054] S5, sintering: preparing the cerium-rich rare earth permanent magnet through vacuum sintering and tempering process on the green body after forming, adopting two-stage tempering process; the first-stage tempering temperature is lower than the second-stage tempering temperature, and the difference between the two tempering temperatures is 120-280°C.

[0055] In the heating exhaust and dehumidification stage, during the heating process, when the temperature is at 100-150°C, it is kept warm for 0.5-1 hour, the sintering temperature is 1020-1080°C, the vacuum degree is less than 0.1Pa, and the time is 4-10 hours; preferably, during the heating process, when the temperature is 120°C, it is kept warm for 1 hour, the sintering temperature is 1080°C, and the vacuum degree is 3×10 -2 , the heat preservation time is 5.5 hours;

[0056] During the sintering process, the primary tempering temperature and the secondary tempering temperature differ by 150-200°C; preferably, the primary tempering temperature is 480°C, the holding time is 4 hours, and the secondary tempering temperature is 640°C, the holding time is 5 hours.

[0057] The performance test of the prepared cerium-rich magnet was performed using a permanent magnet performance measuring instrument at room temperature. Three batches of products were produced using the same process, and the magnetic properties of 5 samples were randomly tested in each batch. The test results are shown in Table 3.

[0058] Table 3 Magnetic properties test results of the magnets prepared in Example 2

[0059] Test heat Remanence(kGs) Coercivity(kOe) Magnetic energy product (MGOe) Squareness(%) 1# 12.48-12.56 15.5-15.9 36.7-37.2 96.2-97.1 2# 12.5-12.58 15.8-16.3 36.9-37.2 96.6-97.4 3# 12.51-12.61 15.9-16.2 37-37.4 97.2-98.0

[0060] Comparative Example 2

[0061] Comparative Example 2 is a cerium-rich magnet prepared by using the same chemical composition and similar process as Example 2, except that a different tempering process is used, specifically: the primary tempering temperature is 750°C, the holding time is 3 hours, and the secondary tempering temperature is 640°C, the holding time is 5 hours. The same process is used to produce three batches of products, and the test method is the same as that of Example 2. The test results are shown in Table 4.

[0062] Table 4 Magnetic properties test results of the magnet prepared in Comparative Example 2

[0063] Test heat Remanence(kGs) Coercivity(kOe) Magnetic energy product (MGOe) Squareness(%) 1# 12.31-12.38 14.2-14.9 36.1-37.2 95.3-96.8 2# 12.18-12.35 15.7-16.5 34.9-36.7 91.8-96.7 3# 12.09-12.27 14.3-15.8 34.2-35.8 92.5-97.1

[0064] It can be seen from the above-mentioned Example 2 and Comparative Example 2 that, under the condition of completely identical chemical composition, compared with the traditional process, the remanence is significantly improved by changing the tempering process, and the difference in remanence, coercive force, magnetic energy product and squareness between furnaces is small, and the magnetic property stability is high. In summary, the present invention can improve the comprehensive magnetic properties of cerium-rich magnets, and has high stability, which is suitable for large-scale production. In addition, the present invention is not limited to cerium-rich magnets, and is also applicable to neodymium iron boron magnets.

[0065] The invention discloses a preparation method for improving the magnetic properties of cerium-rich rare earth permanent magnets. Under the condition that the cerium content and the total amount of rare earth are the same, a certain proportion of Gd is added to the raw materials, so that the coercive force of the magnet can be significantly improved, the remanence is equivalent to that of the method of not adding Gd to the raw materials, and the squareness is higher than that of the method of not adding Gd to the raw materials, and the magnet has higher comprehensive magnetic properties. Under the condition that the chemical composition is completely the same, the remanence is significantly improved by changing the tempering process compared with the traditional process, and the differences in remanence, coercive force, magnetic energy product and squareness between furnaces are small, and the magnetic property stability is high.

[0066] Finally, it should be noted that the above embodiments only illustrate the technical solutions of the present invention, rather than limiting it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A preparation method for improving the magnetic properties of cerium-rich rare earth permanent magnets, characterized in that: The steps include: S1, providing raw materials of cerium-rich rare earth permanent magnets, wherein the cerium-rich magnet composition is Ce by mass percentage. x G y R z Fe 100-x-y-z-b- c M a B b , wherein R is at least one of Nd, Pr, Dy, Tb, and Ho, M is at least one of Co, Al, Cu, Ga, Nb, Zr, and Ti, 6≤x≤16, 0.5≤y≤2, 10≤z≤28, 0.1≤a≤5, 0.85≤c≤0.94, 29≤x+y+x≤33; and 5≤x / y≤10; S2, rapid setting: using rapid setting process to prepare cerium-rich rare earth iron boron alloy rapid setting sheet; S3, powder making: crushing the cerium-rich rare earth iron boron alloy quick-setting flakes into fine powder by hydrogen crushing and air flow milling process; S4, forming: the fine powder after air flow milling is subjected to magnetic field orientation forming and isostatic pressing process to prepare cerium-rich rare earth iron boron alloy green body; S5, sintering: preparing the formed green body into the cerium-rich rare earth permanent magnet through vacuum sintering and tempering process, using a two-stage tempering process; wherein the first-stage tempering temperature is lower than the second-stage tempering temperature, and the two tempering temperatures differ by 120-280°C.

2. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S1, 6≤x / y≤8.

3. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: It is characterized in that In step S2, the maximum melting temperature is 1450-1480°C.

4. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S3, the average particle size of the fine powder is 2.6-3.2 um.

5. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S4, the intensity of the forming magnetic field is 1.5-2.0 T, the oxygen content of the forming press is less than or equal to 300 ppm, and the isostatic pressing pressure is 180-220 MPa.

6. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S5, during the heating process, when the temperature is at 100-150°C, it is kept warm for 0.5-1 hour; during the sintering process, the sintering temperature is 1020-1080°C, the vacuum degree is less than 0.1 Pa, and the time is 4-10 hours.

7. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S5, during the sintering process, the primary tempering temperature is 420-500°C, the tempering time is 2-6 hours, and the secondary tempering temperature is 600-700°C, and the tempering time is 2-6 hours.

8. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S5, the primary tempering temperature and the secondary tempering temperature differ by 150-200°C.

9. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S1, the raw material of cerium-rich rare earth permanent magnet, according to the mass percentage of each component element, has the following specific components: Ce7Gd1Nd 16.7 Pr 5.5 Al 0.1 Cu 0.15 Zr 0.25 Fe 68.38 B 0.92 , where the ratio of Ce to Gd content is 7.

10. The method for preparing a cerium-rich rare earth permanent magnet for improving magnetic properties according to claim 1, characterized in that: In step S1, the raw material of the cerium-rich rare earth permanent magnet is composed of the following components in terms of the mass percentage of each component element: Ce 10 G 1. 6Nd 15.1 Pr 4.8 Al 0.3 Cu 0.2 Zr 0.3 Ti 0.2 Ga 0.15 Fe 66.45 B 0.9 , where the ratio of Ce to Gd content is 6.25.

Citation Information

Patent Citations

  • Gadolinium-containing Nd-Fe-B rare earth permanent magnetic material dn its manufacturing method

    CN101071667A

  • Preparation method for gadolinium-doped permanent magnet material

    CN105931783A

  • Neodymium-iron-boron magnet and preparation method, and neodymium-iron-boron magnet photo frame

    CN106169345A

  • Low-cost N35 NdFeB magnet with high cerium content and sintering method thereof

    CN107610858A

  • Preparation method for improving performance uniformity of cerium-rich magnetic body used for drive motor

    CN108172390A