Grain boundary diffusion preparation process of cerium-containing neodymium iron boron magnetic steel
Through grain boundary diffusion technology and the use of heavy rare earth diffusion agents, the problem of difficult preparation of neodymium iron boron permanent magnets with high residual magnets and high coercive forces is solved, and high performance and low cost magnet preparation is achieved.
Patent Information
- Application Number
- CN202411079024.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-15
AI Technical Summary
It is difficult to prepare sintered NdFeB permanent magnets with high residual magnetism and high coercivity, and heavy rare earths consume a lot and cost high.
By using grain boundary diffusion technology, the main phase alloy and grain boundary alloy are prepared, and the smelting quick-coagulation sheet process, hydrogen crushing treatment, airflow grinding treatment, lubricant and antioxidant are added, and the blank is pressed and sintered and aging heat treatment is carried out. The surface is coated with heavy rare earth diffuser and further heat treatment is performed under an inert atmosphere.
The remanent magnetism and coercivity of neodymium iron boron magnets are improved, the consumption and cost of heavy rare earths are reduced, and the high performance of the magnet is ensured.
Smart Images

Figure CN118969481A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earth magnetic materials, and in particular to a grain boundary diffusion preparation process of cerium-containing neodymium iron boron magnetic steel. Background Art
[0002] NdFeB magnet is a rare earth permanent magnet material with excellent magnetic properties such as high magnetic energy product, high coercive force and high magnetic saturation. It is widely used in motors, instruments, communication equipment and other fields.
[0003] After adding 1% dysprosium by the traditional alloying method, the coercivity increases by about 2-3kOe; after adding 1% terbium, the coercivity increases by 4-6kOe, but the remanence decreases significantly. Sintered NdFeB permanent magnets with high remanence and high coercivity cannot be prepared using traditional alloying methods. In contrast, grain boundary diffusion technology, as an emerging technology, has obvious advantages in cost, heavy rare earth consumption and coercivity improvement. At present, the maturity of grain boundary diffusion technology has become a symbol for evaluating the advancement of NdFeB enterprises. This technology is considered to be an important technological innovation in the sintered NdFeB permanent magnet industry in the 21st century. With the development of strategic emerging fields, the demand for high-performance NdFeB magnets will continue to grow, which puts higher requirements and more urgent needs on grain boundary diffusion technology. Summary of the invention
[0004] The purpose of the present invention is to provide a grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel to solve the problem.
[0005] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, characterized by comprising the following steps:
[0006] Step 1, preparing main phase alloy and grain boundary phase alloy;
[0007] Step 2, using a melting and quick-setting sheet process, melting the main phase alloy in a vacuum melting furnace to obtain a quick-setting sheet;
[0008] Step 3, hydrogen crushing treatment is performed on the rapidly solidified thin slice and the grain boundary phase alloy to obtain hydrogen crushed powder;
[0009] Step 4, jet milling the hydrogen-broken powder and mixing it evenly to obtain magnetic powder;
[0010] Step 5, pressing the magnetic powder into a blank, sintering and performing aging heat treatment to obtain a cerium-containing NdFeB magnetic steel blank;
[0011] Step 6, cleaning and drying the cerium-containing NdFeB magnet blank;
[0012] Step 7, using a spraying technique to coat a heavy rare earth diffusion agent on the surface of the cerium-containing NdFeB magnet blank to obtain a cerium-containing NdFeB magnet semi-finished product;
[0013] Step 8: Perform aging heat treatment on the semi-finished product of cerium-nedymium-iron-boron magnetic steel under an inert atmosphere to obtain cerium-nedymium-iron-boron magnetic steel.
[0014] Furthermore, in step 1, the main phase alloy contains rare earth elements, and at least includes Ce, Pr, Tb and Nd elements.
[0015] Furthermore, in step 1, the grain boundary phase alloy contains Ce, N and F elements.
[0016] Furthermore, in step 1, the grain boundary phase alloy also contains Cu, Al and Zn elements.
[0017] Furthermore, in step 1, the volume ratio of the main phase alloy to the grain boundary phase alloy is 70-80%: 20-30%.
[0018] Furthermore, in step 2, the casting temperature of the smelting furnace is 1400-1500°C, the water temperature of the copper roller is 32-36°C, the rotation speed of the copper roller is 800-1200r / min, and the thickness of the obtained quick-setting sheet is 0.2-0.4mm.
[0019] Furthermore, in step 3, the rapidly solidified thin sheets and grain boundary phase alloys are crushed into 3-4 cm ingots by a 50 t press before hydrogen crushing.
[0020] Furthermore, in step 3, the ingot is placed in a stainless steel pressure tank of a hydrogen crushing device, the pressure tank is evacuated to 22 MPa, 99.6-99.9% pure hydrogen is introduced to 10.5 MPa, the reaction is carried out for 25-30 minutes, and cooling water is introduced for cooling to obtain particles with an average particle size of 1-2 cm.
[0021] Furthermore, in step 4, a lubricant and an antioxidant are added to the magnetic powder during the jet milling process, wherein the lubricant is polyethylene glycol and the antioxidant is thymol.
[0022] Furthermore, the volume proportions of the hydrogen-breaking powder, lubricant and antioxidant are 70-80%: 15-20%: 5-10%.
[0023] Furthermore, in step 4, the particle size of the main phase alloy powder produced by the air flow mill is less than 3 μm, and the particle size of the grain boundary phase alloy powder is less than 3 μm.
[0024] Furthermore, in step 5, the density of the blank is 4.8-5.2 g / m 3The sintering temperature is 800-900℃, the sintering time is 40-60min, then the temperature is raised to 1200-1250℃, kept warm for 3-4h, and then two aging heat treatments are carried out. The first aging temperature is 900-1100℃, the aging time is 5h, and the second aging temperature is 500-700℃, and the aging time is 5h.
[0025] Furthermore, in step 6, the surface of the iron boron magnet sample is first cleaned by grinding it with a grinder, then rinsed with distilled water for 10-15 minutes, ultrasonically cleaned with anhydrous ethanol for 3-5 minutes, and dried at 40-45°C for 55-60 minutes.
[0026] Furthermore, in step 7, the heavy rare earth diffusant is composed of a heavy rare earth metal compound, a solvent, and a binder, and the weight ratio of the heavy rare earth metal compound, the solvent, and the binder is 40-60%: 30-40%: 5-10%.
[0027] Furthermore, in step 8, the inert atmosphere is argon, and two aging heat treatments are performed, the first aging temperature is 900-1100° C., the aging time is 5 hours, and the second aging temperature is 500-700° C., and the aging time is 5 hours.
[0028] A cerium-containing neodymium-iron-boron magnetic steel is prepared by the above-mentioned preparation process.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention relates to a method for adding a lubricant to magnetic powder. By adding a lubricant, the rotational resistance of magnetic particles can be reduced, the orientation degree of the powder can be improved, and the remanence and final magnetic properties of the magnet can be enhanced. In addition, the lubricant is added to the magnetic powder to ensure that the lubricant can be sufficiently rubbed to make the hydrogen powder fine even in the jet mill.
[0031] 2. The present invention controls the thickness of the quick-setting sheet to between 0.2-0.4 mm, which can reduce the precipitation of α-Fe and ensure the volume of the main phase Fe in the magnet. At the same time, reducing the precipitation of α-Fe helps to arrange the crystals in the final finished magnet in a regular manner, promotes the smooth entry of the heavy rare earth diffusant into the grain boundary phase, and thus maximizes the coercive force of the magnet.
[0032] 3. The present invention prepares a layer of heavy rare earth diffusion source on the surface of sintered NdFeB permanent magnet, and then performs aging heat treatment on the permanent magnet under vacuum or inert gas protection. During the heat treatment, the grain boundary phase of sintered NdFeB melts and becomes a liquid phase, and the heavy rare earth elements on the surface of the permanent magnet diffuse into the interior of the permanent magnet through the liquid phase grain boundary channel, and form a heavy rare earth-rich shell layer on the surface of the NdFeB grains. The rich rare earth shell layer has a higher magnetocrystalline anisotropy field than the NdFeB grains, thereby greatly improving the overall coercive force of the sintered NdFeB permanent magnet. Since the heavy rare earth elements are mainly distributed in the grain boundary phase and rarely enter the main phase, the remanence of the sintered NdFeB permanent magnet decreases less, and the heavy rare earth consumption is less, and the cost is lower. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart of a grain boundary diffusion preparation process for a cerium-containing NdFeB magnetic steel according to an embodiment of the present application. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] See also Figure 1 , a grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel, comprising the following steps:
[0037] Step 1, preparing a main phase alloy and a grain boundary phase alloy, with a volume ratio of 70%:30%;
[0038] Step 2: Using a melting and quick-setting sheet process, the main phase alloy is melted in a vacuum melting furnace to obtain a quick-setting thin sheet, wherein the casting temperature of the melting furnace is 1400° C., the water temperature of the copper roller is 32° C., the speed of the copper roller is 800 r / min, and the thickness of the quick-setting thin sheet is 0.2 mm;
[0039] Step 3, hydrogen crushing treatment is performed on the rapidly solidified thin slice and the grain boundary phase alloy to obtain hydrogen crushed powder;
[0040] Step 4, jet milling the hydrogen-crushed powder and mixing it evenly to obtain magnetic powder, wherein the volume proportion of the hydrogen-crushed powder, the lubricant, and the antioxidant is 70%: 20%: 10%;
[0041] Step 5: Press the magnetic powder into a blank, sinter it, and perform aging heat treatment to obtain a cerium-containing NdFeB magnet blank, wherein the blank density is 1.8 g / m 3, sintering temperature is 800℃, sintering time is 40min, holding temperature is 1225℃, holding time is 3.5h, first aging temperature is 900℃, aging time is 5h, second aging temperature is 500℃, aging time is 5h;
[0042] Step 6, cleaning and drying the cerium-containing NdFeB magnet blank;
[0043] Step 7: Use spraying technology to coat the surface of the cerium-containing NdFeB magnet blank with a heavy rare earth diffusion agent to obtain a cerium-containing NdFeB magnet semi-finished product, wherein the weight ratio of the heavy rare earth metal compound, the solvent, and the binder in the heavy rare earth diffusion agent is 50%:40%:10%;
[0044] Step 8: Perform aging heat treatment on the cerium-containing NdFeB semi-finished product under an inert atmosphere to obtain cerium-containing NdFeB magnetic steel, wherein the first aging temperature is 900°C, the aging time is 5 hours, and the second aging temperature is 500°C, and the aging time is 5 hours.
[0045] Example 2
[0046] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 2, the casting temperature of the smelting furnace is 1450°C, the water temperature of the copper roller is 34°C, the rotation speed of the copper roller is 1000r / min, the thickness of the quick-setting sheet obtained is 0.3mm, and the other components and parameters remain unchanged.
[0047] Example 3
[0048] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 2, the casting temperature of the smelting furnace is 1500°C, the water temperature of the copper roller is 36°C, the rotation speed of the copper roller is 1200r / min, the thickness of the quick-setting sheet obtained is 0.4mm, and the other components and parameters remain unchanged.
[0049] Example 4
[0050] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 4, the volume ratios of hydrogen-breaking powder, lubricant and antioxidant are 75%:20%:5%, and the other components and parameters remain unchanged.
[0051] Example 5
[0052] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 4, the volume ratio of hydrogen-breaking powder, lubricant and antioxidant is 80%:15%:5%, and the other components and parameters remain unchanged.
[0053] Example 6
[0054] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that the blank density in step 5 is 5g / m 3 , the sintering temperature is 850℃, the sintering time is 50min, the first aging temperature is 1000℃, the aging time is 5h, the second aging temperature is 600℃, the aging time is 5h, and the other components and parameters remain unchanged.
[0055] Example 7
[0056] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that the density of the blank in step 5 is 5.2 g / m 3 , the sintering temperature is 900℃, the sintering time is 60min, the first aging temperature is 1100℃, the aging time is 5h, the second aging temperature is 700℃, the aging time is 5h, and the other components and parameters remain unchanged.
[0057] Example 8
[0058] A grain boundary diffusion preparation process for cerium-containing NdFeB magnets, the process flow of which is the same as that of Example 1, except that in step 7, the mass proportions of the medium rare earth metal compound, the solvent and the binder in the heavy rare earth diffusant are 60%:30%:10%, and the other components and parameters remain unchanged.
[0059] Example 9
[0060] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 8, the first aging temperature is 1000°C, the aging time is 5 hours, the second aging temperature is 600°C, the aging time is 5 hours, and the other components and parameters remain unchanged.
[0061] Example 10
[0062] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that in step 8, the first aging temperature is 1100°C, the aging time is 5 hours, the second aging temperature is 700°C, the aging time is 5 hours, and the other components and parameters remain unchanged.
[0063] Comparative Example 1
[0064] A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, the process flow of which is the same as that of Example 1, except that step 7 is omitted, and the remaining components and parameters remain unchanged.
[0065] The magnet properties of the above different embodiments and comparative examples were tested at 25° C. The test results are shown in Table 1.
[0066] Table 1
[0067]
[0068] It can be seen from Table 1 that the remanence of the magnetic steel prepared by the grain boundary diffusion preparation process of the cerium-containing NdFeB magnetic steel adopted in the present invention reaches 13.2-13.8, the coercive force is ≥12.6, and the maximum magnetic energy product reaches 43-46.
[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, characterized in that: The following steps are involved: Step 1, preparing main phase alloy and grain boundary phase alloy; Step 2, using a melting and quick-setting sheet process, melting the main phase alloy in a vacuum melting furnace to obtain a quick-setting thin sheet; Step 3, hydrogen crushing treatment is performed on the rapidly solidified thin slice and the grain boundary phase alloy to obtain hydrogen crushed powder; Step 4, jet milling the hydrogen-broken powder and mixing it evenly to obtain magnetic powder; Step 5, pressing the magnetic powder into a blank, sintering and performing aging heat treatment to obtain a cerium-containing NdFeB magnetic steel blank; Step 6, cleaning and drying the cerium-containing NdFeB magnet blank; Step 7, using a spraying technique to coat a heavy rare earth diffusion agent on the surface of the cerium-containing NdFeB magnet blank to obtain a cerium-containing NdFeB magnet semi-finished product; Step 8: Perform aging heat treatment on the cerium-containing NdFeB semi-finished product under an inert atmosphere to obtain cerium-containing NdFeB magnetic steel.
2. The grain boundary diffusion preparation process of a cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In the step 1, the main phase alloy contains Fe and B; in the step 1, the main phase alloy also contains rare earth elements, and at least includes Ce, Pr, Tb and Nd elements; in the step 1, the grain boundary phase alloy contains Ce, N and F elements; in the step 1, the grain boundary phase alloy also contains Cu, Al and Zn elements; in the step 1, the volume ratio of the main phase alloy and the grain boundary phase alloy is 70-80%:20-30%.
3. The grain boundary diffusion preparation process of a cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In the step 2, the casting temperature of the smelting furnace is 1400-1500° C., the water temperature of the copper roller is 32-36° C., the rotation speed of the copper roller is 800-1200 r / min, and the thickness of the obtained quick-setting sheet is 0.2-0.4 mm.
4. The grain boundary diffusion preparation process of a cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In the step 3, the quick-solidified thin sheet and the grain boundary phase alloy are crushed into 3-4 cm ingots by a 50t press before hydrogen crushing treatment; in the step 3, the ingots are placed in a stainless steel pressure tank of a hydrogen crushing device, the pressure tank is evacuated to 22MPa, 99.6-99.9% purity hydrogen is introduced to 10.5MPa, the reaction is carried out for 25-30 minutes, and cooling water is introduced for cooling to obtain particles with an average particle size of 1-2cm.
5. The grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In the step 4, a lubricant and an antioxidant are added to the magnetic powder during the air flow milling process, wherein the lubricant is polyethylene glycol and the antioxidant is thymol; the volume proportions of the hydrogen-crushed powder, the lubricant and the antioxidant are 70-80%: 15-20%: 5-10%; in the step 4, the particle size of the main phase alloy powder ground by the air flow mill is <3μm, and the particle size of the grain boundary phase alloy powder is <3μm.
6. The grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In step 5, the blank density is 4.8-5.2g / m 3 The sintering temperature is 800-900℃, the sintering time is 40-60min, then the temperature is raised to 1200-1250℃, kept warm for 3-4h, and then two aging heat treatments are carried out. The first aging temperature is 900-1100℃, the aging time is 5h, and the second aging temperature is 500-700℃, and the aging time is 5h.
7. The grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In step 6, the surface of the iron boron magnet sample is first cleaned by grinding with a grinder, then rinsed with distilled water for 10-15 minutes, ultrasonically cleaned with anhydrous ethanol for 3-5 minutes, and dried at 40-45° C. for 55-60 minutes.
8. The grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In step 7, the heavy rare earth diffuser is composed of a heavy rare earth metal compound, a solvent, and a binder, and the weight ratio of the heavy rare earth metal compound, the solvent, and the binder is 40-60%: 30-40%: 5-10%.
9. The grain boundary diffusion preparation process of cerium-containing NdFeB magnetic steel according to claim 1, characterized in that: In step 8, the inert atmosphere is argon, and two aging heat treatments are performed, the first aging temperature is 900-1100° C., the aging time is 5 hours, and the second aging temperature is 500-700° C., and the aging time is 5 hours.
10. A grain boundary diffusion preparation process for cerium-containing NdFeB magnetic steel, characterized in that: Prepared by the process described in any one of claims 1 to 16.
Citation Information
Cited By
Process for preparing high-comprehensive-performance and high-abundance cerium magnet through grain boundary diffusion