Flash spinning fiber containing organic pigment as well as preparation method and application of flash spinning fiber
By wrapping and processing organic pigments in flash spinning technology and introducing polar substituted groups, the problem of pigment deterioration during spinning is solved, and the light resistance, friction resistance and soap washing resistance of spinning fibers are improved, ensuring that the product is Stability and strength in high temperature and high pressure environments.
Patent Information
- Application Number
- CN202411207826.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
Flash Spinning products are prone to deterioration when using organic pigments in high temperature and high pressure environments, resulting in fiber products not resistant to light, soap washing and fading easily. The pigment has poor uniformity on the fiber surface, affecting breathability and durability.
After adjusting the particle size of the organic pigment to 300 nm to 500 nm and wrapping in polyaryl sulfone, polar substituent groups are introduced in combination with hydroxyethyl acrylate to form a modified pigment and added to the spinning liquid to improve the temperature resistance of the pigment. , pressure and solvent resistance properties to ensure the stability of the pigment during spinning.
It improves the light resistance, friction resistance and soap washing resistance of spinned fibers, and the color fastness reaches level 4 or above, ensuring the stability and strength of fiber products in high temperature and high pressure environments, and extending the service life.
Smart Images

Figure BDA0005019531000000061 
Figure BDA0005019531000000121
Abstract
Description
Technical Field
[0001] The present application relates to the field of spinning technology, and in particular to a flash-spun fiber containing an organic pigment, and a preparation method and application thereof. Background Art
[0002] Flash spinning, also known as instant spinning, is a spinning method in which a polymer solution is released through the spinneret of a flash spinning device under high temperature and high pressure into an environment of normal temperature and pressure. Due to the sudden drop in pressure, the low-boiling point solvent vaporizes rapidly and evaporates instantly, while the polymer solidifies rapidly from the liquid state and is stretched by the high-speed solvent gas to form fibers. Flash spinning technology was first successfully developed by DuPont in the United States in 1957. The polyethylene material prepared by the flash spinning method has excellent strength, waterproofness, and breathability, and has been widely used in many fields such as medicine, packaging, and construction.
[0003] In the production process of flash spinning, undyed raw materials are directly made through spinning, web forming, reinforcement and other processes. Therefore, its original color is usually white or close to the color of the fiber itself. It needs to be printed and dyed with pigments to present a specific color. However, the printing and dyeing agents in the printing and dyeing process will accumulate between the pores of the fibers, thereby affecting the air permeability and durability of the flash-spun nonwoven fabrics themselves, limiting the application of flash-spun nonwoven fabrics. In order to make the flash spinning process smoother or give the product certain specific properties, other additives such as nucleating agents, stabilizers, antioxidants, expanders, dyes and pigments can also be added to the spinning solution. For example, in the latest study by Harris et al., pigments were added to polyethylene to make the flash-spun nonwoven sheet have better printing properties.
[0004] However, due to the special fiber structure and surface properties of flash spinning products, the pigments added during the production process may be difficult to penetrate evenly and firmly adhere to the fiber surface, resulting in the problem of easy fading after washing or friction. In addition, organic pigments have the advantages of bright and obvious colors, complete color spectrum, and high coloring power, but organic pigments have low temperature resistance, most of which are below 200°C. In the production process of flash spinning, the spinning solution needs to be treated in a high temperature and high pressure environment for a long time. Organic pigments are subject to multiple influences of temperature, pressure, and spinning solvents during the flash spinning process, and are prone to deterioration, resulting in the prepared fiber products being not resistant to light, soap washing, etc., and are prone to fading or discoloration. Summary of the invention
[0005] The present application provides a flash-spun fiber containing an organic pigment, and a preparation method and application thereof. By treating the organic pigment to improve its temperature resistance, pressure resistance, and solvent resistance, the organic pigment is effectively prevented from deteriorating during the flash spinning preparation process, thereby ensuring the strength and toughness of the flash-spun fiber product itself, while improving its light resistance, wash resistance, and friction resistance.
[0006] In order to solve the above technical problems, one of the purposes of the present application is to provide a method for preparing flash-spun fibers containing organic pigments, comprising the following steps:
[0007] The polyarylsulfone is heated and dissolved in solvent A, and then an organic pigment and a dispersant are added to obtain a mixed solution A, wherein the particle size of the organic pigment is greater than or equal to 300 nm and less than or equal to 500 nm, and the solution is homogenized and stirred, and then filtered to obtain the encapsulated pigment.
[0008] The wrapped pigment is heat treated in an oxygen-proof manner at a temperature greater than or equal to 150° C. and less than or equal to 180° C., and then cooled to obtain a treated pigment.
[0009] The treated pigment is placed in a solvent B containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added to obtain a mixed solution B. After stirring for reaction, the solution is filtered and dried to obtain a modified pigment.
[0010] The polymer melt and the modified pigment are mixed to form a uniform polymer mixture, the spinning solvent is mixed to form a uniform solvent mixture, the polymer mixture and the solvent mixture are mixed in a mixing device, heated and nitrogen is introduced, so that the temperature in the mixing device is greater than or equal to 200° C. and less than or equal to 220° C., and the pressure is greater than or equal to 10 MPa and less than or equal to 13 MPa, and the mixture is stirred in a closed state, and a spinning solution is obtained after the temperature and pressure are stabilized.
[0011] The spinning solution is ejected through the spinneret holes of the connected flash spinning equipment, stretched and opened by an air amplifier to form an ultrafine fiber web, which is then laid on a mobile device and subjected to cold pressing and hot rolling to obtain a fiber sheet.
[0012] The spinning solution comprises 16wt%-20wt% of polymer melt, 0.5wt%-1.5wt% of modified pigment, 0wt%-5wt% of additive and the balance of spinning solvent.
[0013] By adopting the above scheme, the present application adds modified pigments to the spinning solution, utilizing the high temperature resistance and transparency of polyarylsulfone itself. The organic pigment is pre-wrapped with polyarylsulfone to form a heat-resistant layer, which will not block the color of the organic pigment itself. After high-temperature heat treatment, the crystallinity and orientation of the polymer heat-resistant layer can be maximized, thereby enhancing its high-temperature resistance and rigidity, so that the heat and pressure resistance of the pigment can adapt to the high temperature and high pressure environment of the spinning process. At the same time, the heat-resistant layer is combined with hydroxyethyl acrylate to introduce a large number of polar substituent groups, which can improve the solvent resistance of the modified pigment and avoid the polyarylsulfone heat-resistant layer from being affected by the spinning solvent in a long-term high-temperature environment and dissolving and rupture. The modified pigment has a low degree of deterioration after long-term high-temperature flash spinning production, and the light resistance, friction resistance and soap washing color fastness of the finally prepared fiber product can reach above level 4, and it is not easy to fade or discolor.
[0014] In addition, by controlling the particle size of the organic pigment in the spinning solution and the amount of modified pigment added, the present application can ensure that the modified pigment is evenly dispersed in the spun fiber and the particles are small, thereby ensuring that the flash spun fiber product can achieve higher strength and toughness and meet the application performance requirements.
[0015] As a preferred embodiment, the mixed solution A includes 4wt%-7wt% polyarylsulfone, 10wt%-18wt% organic pigment, 1wt%-2wt% dispersant and the balance solvent A.
[0016] As a preferred embodiment, the mixed solution B includes 15wt%-20wt% of treated pigment, 3wt%-8wt% of hydroxyethyl acrylate, 1wt%-3wt% of 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the balance of solvent B.
[0017] As a preferred embodiment, the mass ratio of the polymer melt to the modified pigment is (16-32):1.
[0018] By adopting the above scheme, the present application controls the mass ratio of polymer melt and modified pigment to be between (16-32):1, which can ensure that the prepared fiber product itself has high strength and toughness, avoid the addition of modified fillers affecting the fiber properties, and the fiber sheets have high resistance to friction, soaping and light, and the color fastness reaches above level 4, which can expand the application field.
[0019] As a preferred embodiment, the speed of homogenizing and stirring the mixed solution A is greater than or equal to 600 rpm and less than or equal to 800 rpm.
[0020] As a preferred embodiment, the time for heat treatment of the encapsulated pigment is greater than or equal to 20 minutes and less than or equal to 30 minutes.
[0021] As a preferred embodiment, the reaction time of the mixed solution B is greater than or equal to 1 h and less than or equal to 3 h.
[0022] As a preferred embodiment, the closed stirring time of the mixing equipment is greater than or equal to 2 hours and less than or equal to 3 hours.
[0023] As a preferred solution, the air flow rate of the spinneret of the flash spinning equipment is greater than or equal to 10000 m / min and less than or equal to 13000 m / min, and the spinneret aperture is greater than or equal to 1 μm and less than or equal to 5 μm.
[0024] As a preferred embodiment, the organic pigment is at least one of phthalocyanine red, phthalocyanine blue, phthalocyanine green, permanent yellow, permanent violet and azo red.
[0025] As a preferred embodiment, the organic pigment includes at least one of CIRR53:1, CIRR48:1, CIRR48:2, CIRR48:3, CIRR170, CIRR21, CIRR104, CIRR57:1, CIRY14, CIRY 12, CIRY83, CIRY 13, CIRY 1, CIRY3, CIRO13, CIRO34, and CIRV23.
[0026] As a preferred embodiment, the polymer melt is at least one of polyesters such as polyethylene, high-density polyethylene, polypropylene, polybutene, polymethylpentene, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, PET, and polylactic acid.
[0027] As a preferred embodiment, the polymer melt is high density polyethylene.
[0028] As a preferred embodiment, the melt index of the high-density polyethylene at 190°C and 2.16 load is 5-12 g / 10 min.
[0029] As a preferred embodiment, solvent A is at least one of dimethylformamide, dimethyl sulfoxide and N-methylpyrrolidone.
[0030] As a preferred embodiment, the dispersant is at least one of sodium dodecylbenzene sulfonate, polyvinyl alcohol, pyrrolidone, and sodium methylene dinaphthalene sulfonate.
[0031] As a preferred embodiment, solvent B is an aliphatic hydrocarbon solvent.
[0032] As a preferred embodiment, solvent B is at least one of butane, pentene, n-hexane, heptane and octane.
[0033] By adopting the above scheme, the treated pigment of the present application is pre-wrapped with polyarylsulfone on the surface of the organic pigment to form a heat-resistant layer. The surface of polyarylsulfone has fewer polar groups and limited solvent resistance. The use of aliphatic hydrocarbon solvents can improve the stability of the heat-resistant layer and avoid cracking of the heat-resistant layer.
[0034] As a preferred embodiment, the spinning solvent is at least one of toluene, benzene, n-hexane, butane, pentene, heptane, octane, cyclohexane, cyclopentane, dichloromethane, carbon tetrachloride, chloroform, chloromethane, ethyl chloride, dichloroethylene, trichlorofluoromethane, dichlorotrifluoroethane, pentafluoropropane, heptafluoropropane, perfluorohexane, perfluorohexane, perfluoroheptane, octafluorocyclopentane, and alcohol solvents.
[0035] As a preferred embodiment, the additive is at least one of a nucleating agent, a stabilizer, an antioxidant, a swelling agent, and an antibacterial agent.
[0036] In order to solve the above technical problems, the second purpose of the present application is to provide a flash spun fiber containing an organic pigment.
[0037] In order to solve the above technical problems, the third purpose of the present application provides an application of a flash-spun fiber containing an organic pigment in the preparation of cultural and creative printed materials, clothing or household products.
[0038] As a preferred solution, the flash-spun fiber nonwoven fabric is combined with cultural and creative printed products, clothing or household products by at least one of interlocking, bonding, heat sealing and sewing. As a preferred solution, the cultural and creative printed products include but are not limited to at least one of canvas bags, stickers, refrigerator magnets and hand-torn books.
[0039] As a preferred solution, the household product includes but is not limited to at least one of a luggage bag, a storage bag, a seat cover, a carpet, a mattress, a door curtain, and an umbrella.
[0040] As a preferred solution, multiple layers of non-woven fabrics of different colors are laminated and welded together, and the mixed colors of the multiple layers of non-woven fabrics are seen through the transparent first sheet or the second sheet to present a beautiful and deep mixed color gradient effect.
[0041] As a preferred solution, the heat-pressing roller of the non-woven fabric welding process performs heat-pressing welding at a temperature of 150° C. or higher and 180° C. or lower.
[0042] The non-woven fabric formed by the flash-spun fibers of the present application can present bright colors due to the addition of organic pigments during the flash spinning process. The non-woven fabric has high color fastness to light, color fastness to soap washing and color fastness to friction, and can withstand light, water washing and high temperature environments. The strength and toughness of the non-woven fabric itself are also maintained. When used in cultural and creative prints, clothing or household products, the non-woven fabric can withstand steam sterilization, high-temperature disinfection, mechanical processing and other treatments. The non-woven fabric will not fade or discolor and has a long service life. In addition, corresponding colors can be designed according to cultural and creative prints, clothing or household products and corresponding organic pigments can be added. The flash-spun non-woven fabric can present the designed color without subsequent printing and dyeing treatment. The removal of printing and dyeing treatment can ensure the air permeability and performance of the flash-spun non-woven fabric itself, reduce the impact of process processing on the performance of the non-woven fabric, save printing and dyeing treatment operations, and have economic benefits.
[0043] Compared with the prior art, this application has the following beneficial effects:
[0044] 1. The present application adds modified pigments to the spinning solution for flash spinning, utilizing the high temperature resistance and transparency of polyarylsulfone itself. The organic pigment is pre-wrapped with polyarylsulfone to form a heat-resistant layer, which will not block the color of the organic pigment itself. After high-temperature heat treatment, the crystallinity and orientation of the polymer heat-resistant layer can be maximized, thereby enhancing its high temperature resistance and rigidity, so that the pigment's heat and pressure resistance can adapt to the high temperature and high pressure environment of the spinning process, effectively avoiding the degradation of the organic pigment during the flash spinning preparation process, improving the light resistance and soap washing resistance of the spun fiber, and not prone to fading or discoloration.
[0045] 2. The organic pigment of the present application is pre-wrapped with polyarylsulfone to form a heat-resistant layer. The heat-resistant layer is combined with hydroxyethyl acrylate to introduce a large number of polar substituent groups, which can improve the solvent resistance of the modified pigment and prevent the polyarylsulfone heat-resistant layer from being dissolved and broken by the spinning solvent in a long-term high-temperature environment. The degree of deterioration of the modified pigment after long-term high-temperature flash spinning production is low. The light resistance, friction resistance and soap washing color fastness of the finally prepared fiber product can reach above level 4, and it is not easy to fade or discolor.
[0046] 3. This application ensures that the modified pigment is evenly dispersed in the spun fiber and has small particles by controlling the particle size of the organic pigment in the spinning solution and the amount of modified pigment added, thereby ensuring that the flash spun fiber product can achieve higher strength and toughness and meet the application performance requirements. DETAILED DESCRIPTION
[0047] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0048] Table 1 - Sources of raw materials in the examples and comparative examples of the present application
[0049]
[0050] Example 1
[0051] A flash spun fiber containing an organic pigment, the preparation method of which comprises the following steps:
[0052] (1) Add polyarylsulfone to a container containing dimethylformamide solvent, heat in a water bath at 60°C and stir to dissolve, then add red organic pigment CIRR53:1 and sodium methylene dinaphthalene sulfonate dispersant, the particle size of the red organic pigment CIRR53:1 is 300nm, and the mass fraction concentration of each component added in the solution is 5wt% polyarylsulfone, 15wt% red organic pigment CIRR53:1, 1wt% sodium methylene dinaphthalene sulfonate dispersant and the balance dimethylformamide, and homogenize and stir for 2h at a homogenization stirring rate of 800rpm, and filter to obtain the encapsulated pigment.
[0053] (2) The coated pigment is placed in a nitrogen furnace to isolate oxygen and heat-treat at 150° C. for 30 min, followed by cooling to obtain a treated pigment.
[0054] (3) The treated pigment is placed in a n-hexane solvent containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added. The mass fraction concentration of each component in the solution is 20wt% treated pigment, 8wt% hydroxyethyl acrylate, 3wt% 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the remainder n-hexane. The reaction is stirred for 1 hour at a stirring rate of 400rpm. After filtering, it is dried at 50°C to obtain a modified pigment.
[0055] (4) High-density polyethylene (HDPE) accounting for 16 wt% of the spinning solution and 0.5 wt% of the modified pigment are transported from the solid storage system to a pretreatment tank through a solid automatic weighing system, and the mass ratio of HDPE to the modified pigment is 32:1, so as to form a uniform polymer mixture. Normal hexane (55 wt% of the spinning solution) and perfluorohexane (26 wt% of the spinning solution) are transported to another pretreatment tank through a liquid automatic weighing system, so as to obtain a uniform solvent mixture.
[0056] (5) The polymer mixture and the solvent mixture are mixed in a mixing kettle, preheated to 160° C., then nitrogen is introduced, pressurized to 12 MPa, and then heated to 220° C. and stirred in a closed state for 2 h. After the temperature and pressure are stabilized, a spinning solution is obtained.
[0057] (6) The spinning solution is ejected through the spinneret holes of the connected flash spinning equipment, the solvent is vaporized in a normal temperature and pressure environment, and the polymer is pulled by the steam to form an ultrafine fiber bundle. The ejection air flow rate is 10000 m / min, and the spinneret hole diameter is 3 μm. The ultrafine fiber bundle is guided to the air amplifier through a steering device, stretched and opened by high-pressure air to form an ultrafine fiber web, which is then laid on a moving mesh curtain and then cold pressed and hot rolled to obtain a fiber sheet.
[0058] Example 2
[0059] A flash spun fiber containing an organic pigment, the preparation method of which comprises the following steps:
[0060] (1) Add polyarylsulfone to a container containing dimethyl sulfoxide solvent, heat in a water bath at 60°C and stir to dissolve, then add red organic pigment CIRR53:1 and sodium dodecylbenzene sulfonate dispersant, the particle size of the red organic pigment CIRR53:1 is 300nm, the mass fraction concentration of each component added in the solution is 7wt% polyarylsulfone, 18wt% red organic pigment CIRR53:1, 2wt% sodium dodecylbenzene sulfonate dispersant and the balance dimethyl sulfoxide, and homogenize and stir for 3h at a homogenization stirring rate of 1000rpm, and filter to obtain the encapsulated pigment.
[0061] (2) The coated pigment is placed in a nitrogen furnace to isolate oxygen and heat-treat at 160° C. for 20 min, followed by cooling to obtain a treated pigment.
[0062] (3) The treated pigment is placed in a n-hexane solvent containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added. The mass fraction concentration of each component in the solution is 15wt% treated pigment, 5wt% hydroxyethyl acrylate, 2wt% 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the remainder n-hexane. The reaction is stirred for 2h at a stirring rate of 400rpm. After filtering, it is dried at 60°C to obtain a modified pigment.
[0063] (4) High-density polyethylene (HDPE) accounting for 18 wt% of the spinning solution and 1 wt% of the modified pigment are transported from the solid storage system to a pretreatment tank through a solid automatic weighing system, and the mass ratio of high-density polyethylene to modified pigment is 18:1, so as to form a uniform polymer mixture. Cyclohexane (52 wt% of the spinning solution) and perfluorohexane (29 wt% of the spinning solution) are transported to another pretreatment tank through a liquid automatic weighing system to obtain a uniform solvent mixture.
[0064] (5) The polymer mixture and the solvent mixture are mixed in a mixing kettle, preheated to 180° C., then nitrogen is introduced, pressurized to 10 MPa, and then heated to 210° C. and stirred in a closed state for 3 h. After the temperature and pressure are stabilized, a spinning solution is obtained.
[0065] (6) The spinning solution is ejected through the spinneret of the connected flash spinning equipment, the solvent is vaporized in a normal temperature and pressure environment, and the polymer is pulled by the steam to form an ultrafine fiber bundle. The ejection air flow rate is 12000m / min, and the spinneret aperture is 3μm. The ultrafine fiber bundle is guided to the air amplifier through a steering device. The air flow speed of the air amplifier is 13000m / min. The ultrafine fiber web is formed by high-pressure air stretching and laying on a moving mesh curtain, and then cold pressed and hot rolled to obtain a fiber sheet.
[0066] Example 3
[0067] A flash spun fiber containing an organic pigment, the preparation method of which comprises the following steps:
[0068] (1) Add polyarylsulfone to a container containing N-methylpyrrolidone solvent, heat in a water bath at 70°C and stir to dissolve, then add red organic pigment CIRR53:1 and sodium methylene dinaphthalene sulfonate dispersant, the particle size of the red organic pigment CIRR53:1 is 300nm, and the mass fraction concentration of each component added in the solution is 4wt% polyarylsulfone, 10wt% red organic pigment CIRR53:1, 1wt% sodium methylene dinaphthalene sulfonate dispersant and the balance dimethyl sulfoxide, and homogenize and stir for 1h at a homogenization stirring rate of 600rpm, and filter to obtain the encapsulated pigment.
[0069] (2) The coated pigment is placed in a nitrogen furnace to isolate oxygen and heat-treat at 180° C. for 20 min, followed by cooling to obtain a treated pigment.
[0070] (3) The treated pigment is placed in a n-hexane solvent containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added. The mass fraction concentration of each component in the solution is 18wt% treated pigment, 3wt% hydroxyethyl acrylate, 1wt% 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the remainder n-hexane. The reaction is stirred for 3h at a stirring rate of 400rpm. After cooling and filtering, the solution is dried at 60°C to obtain a modified pigment.
[0071] (4) High-density polyethylene (HDPE) accounting for 20 wt% of the spinning solution and 1.5 wt% of the modified pigment are transported from the solid storage system to the pretreatment tank through the solid automatic weighing system. The mass ratio of HDPE to the modified pigment is 13:1, forming a uniform polymer mixture. Dichloromethane (58 wt% of the spinning solution) and 20.5 wt% of cyclopentane are transported to another pretreatment tank through the liquid automatic weighing system to obtain a uniform solvent mixture.
[0072] (5) The polymer mixture and the solvent mixture are mixed in a mixing kettle, preheated to 180° C., then nitrogen is introduced, pressurized to 10 MPa, and then heated to 210° C. and stirred in a closed state for 3 h. After the temperature and pressure are stabilized, a spinning solution is obtained.
[0073] (6) The spinning solution is ejected through the spinneret of the connected flash spinning equipment, the solvent is vaporized in a normal temperature and pressure environment, and the polymer is pulled by the steam to form an ultrafine fiber bundle. The ejection air flow rate is 12000m / min, and the spinneret aperture is 3μm. The ultrafine fiber bundle is guided to the air amplifier through a steering device. The air flow speed of the air amplifier is 13000m / min. The ultrafine fiber web is formed by high-pressure air stretching and laying on a moving mesh curtain, and then cold pressed and hot rolled to obtain a fiber sheet.
[0074] Example 4
[0075] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (1), the particle size of the red organic pigment CIRR53:1 is 500 nm.
[0076] Example 5
[0077] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (4), high-density polyethylene accounts for 16wt% of the mass fraction of the spinning solution, and the modified pigment accounts for 1wt% of the mass fraction of the spinning solution, and the mass ratio of high-density polyethylene to the modified pigment is 16:1.
[0078] Example 6
[0079] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (4), high-density polyethylene accounts for 16wt% of the mass fraction of the spinning solution, and the modified pigment accounts for 1.5wt% of the mass fraction of the spinning solution, and the mass ratio of high-density polyethylene to modified pigment is 10.6:1.
[0080] Comparative Example 1
[0081] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (1), the particle size of the red organic pigment CIRR53:1 is 800 nm.
[0082] Comparative Example 2
[0083] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (4), high-density polyethylene accounts for 16wt% of the mass fraction of the spinning solution, the modified pigment accounts for 2wt% of the mass fraction of the spinning solution, and the mass ratio of high-density polyethylene to the modified pigment is 8:1.
[0084] Comparative Example 3
[0085] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (4), the modified pigment is replaced by an equal amount of n-hexane.
[0086] Comparative Example 4
[0087] A flash spun fiber containing an organic pigment, wherein each step and the reagents, equipment and process parameters used in each step are the same as those in Example 1, except that in step (4), an equal amount of the modified pigment is replaced by an untreated red organic pigment CIRR53:1, and the particle size of the red organic pigment CIRR53:1 is 300 nm.
[0088] Comparative Example 5
[0089] A flash spun fiber containing an organic pigment, the preparation method of which comprises the following steps:
[0090] (1) Add polyarylsulfone to a container containing dimethylformamide solvent, heat in a water bath at 60°C and stir to dissolve, then add red organic pigment CIRR53:1 and sodium methylene dinaphthalene sulfonate dispersant, the particle size of the red organic pigment CIRR53:1 is 300nm, and the mass fraction concentration of each component added in the solution is 5wt% polyarylsulfone, 15wt% red organic pigment CIRR53:1, 1wt% sodium methylene dinaphthalene sulfonate dispersant and the balance dimethylformamide, and homogenize and stir for 2h at a homogenization stirring rate of 800rpm, and filter to obtain the encapsulated pigment.
[0091] (2) The coated pigment is placed in a nitrogen furnace to isolate oxygen and heat-treat at 150° C. for 30 min, followed by cooling to obtain a treated pigment.
[0092] (3) High-density polyethylene (HDPE) accounting for 16 wt% of the spinning solution and 0.5 wt% of the treated pigment are transported from the solid storage system to a pretreatment tank through a solid automatic weighing system, wherein the mass ratio of HDPE to the treated pigment is 32:1, to form a uniform polymer mixture. Normal hexane (55 wt% of the spinning solution) and perfluorohexane (26 wt% of the spinning solution) are transported to another pretreatment tank through a liquid automatic weighing system to obtain a uniform solvent mixture.
[0093] (4) The polymer mixture and the solvent mixture are mixed in a mixing kettle, preheated to 160° C., then nitrogen is introduced, pressurized to 12 MPa, and then heated to 220° C. and stirred in a closed state for 2 h. After the temperature and pressure are stabilized, a spinning solution is obtained.
[0094] (5) The spinning solution is ejected through the spinneret holes of the connected flash spinning equipment, the solvent is vaporized in a normal temperature and pressure environment, and the polymer is pulled by the steam to form an ultrafine fiber bundle. The ejection air flow rate is 10000 m / min, and the spinneret hole diameter is 3 μm. The ultrafine fiber bundle is guided to the air amplifier through a steering device, stretched and opened by high-pressure air to form an ultrafine fiber web, which is then laid on a moving mesh curtain and then cold pressed and hot rolled to obtain a fiber sheet.
[0095] Comparative Example 6
[0096] A flash spun fiber containing an organic pigment, the preparation method of which comprises the following steps:
[0097] (1) Add polyarylsulfone to a container containing dimethylformamide solvent, heat in a water bath at 60°C and stir to dissolve, then add red organic pigment CIRR53:1 and sodium methylene dinaphthalene sulfonate dispersant, the particle size of the red organic pigment CIRR53:1 is 300nm, and the mass fraction concentration of each component added in the solution is 5wt% polyarylsulfone, 15wt% red organic pigment CIRR53:1, 1wt% sodium methylene dinaphthalene sulfonate dispersant and the balance dimethylformamide, and homogenize and stir for 2h at a homogenization stirring rate of 800rpm, and filter to obtain the encapsulated pigment.
[0098] (2) The coated pigment is placed in a n-hexane solvent containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added. The mass fraction concentration of each component in the solution is 20wt% of the coated pigment, 8wt% of hydroxyethyl acrylate, 3wt% of 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the remainder of n-hexane. The reaction is stirred for 1 hour at a stirring rate of 400rpm. After filtering, the modified pigment is dried at 50°C to obtain a modified pigment.
[0099] (3) High-density polyethylene (HDPE) accounting for 16 wt% of the spinning solution and 0.5 wt% of the modified pigment are transported from the solid storage system to a pretreatment tank through a solid automatic weighing system, and the mass ratio of high-density polyethylene to the modified pigment is 32:1, forming a uniform polymer mixture. Normal hexane (55 wt% of the spinning solution) and perfluorohexane (26 wt% of the spinning solution) are transported to another pretreatment tank through a liquid automatic weighing system to obtain a uniform solvent mixture.
[0100] (4) The polymer mixture and the solvent mixture are mixed in a mixing kettle, preheated to 160° C., then nitrogen is introduced, pressurized to 12 MPa, and then heated to 220° C. and stirred in a closed state for 2 h. After the temperature and pressure are stabilized, a spinning solution is obtained.
[0101] (5) The spinning solution is ejected through the spinneret holes of the connected flash spinning equipment, the solvent is vaporized in a normal temperature and pressure environment, and the polymer is pulled by the steam to form an ultrafine fiber bundle. The ejection air flow rate is 10000 m / min, and the spinneret hole diameter is 3 μm. The ultrafine fiber bundle is guided to the air amplifier through a steering device, stretched and opened by high-pressure air to form an ultrafine fiber web, which is then laid on a moving mesh curtain and then cold pressed and hot rolled to obtain a fiber sheet.
[0102] In order to verify the performance of the flash-spun fibers of the present application, the products prepared in the embodiments and comparative examples were subjected to the following performance tests, and the specific steps are as follows:
[0103] (1) Nail rod tear strength: The fiber sheets of the embodiment and the comparative example were tested for nail rod tear strength according to GB / T328.18 standard. The test results are shown in Table 1 below.
[0104] (2) Tensile strength: The tensile strength of the fiber sheets of the embodiment and the comparative example was tested according to GB / T12914 standard. The test results are shown in Table 1 below.
[0105] (3) Color fastness to rubbing: The color fastness to rubbing of the fiber sheets of the embodiment and the comparative example was evaluated in accordance with GB / T3920 "Textiles - Color Fastness - Color Fastness to Rubbing", with the grades ranging from 1 to 5. The lower the grade, the more serious the fading. The evaluation results are shown in Table 1 below.
[0106] (4) Color fastness to washing with soap: The color fastness to washing with soap of the fiber sheets of the embodiment and the comparative example was evaluated in accordance with GB / T3921 "Color fastness of textiles - Color fastness to washing with soap" on a scale of 1-5, where a lower grade indicates more severe fading. The evaluation results are shown in Table 1 below.
[0107] (5) Color fastness to light: The color fastness to light of the fiber sheets of the embodiment and the comparative example was evaluated in accordance with GB / T8427 "Textiles - Color fastness - Color fastness to artificial light". The grades are 1-5, and the lower the grade, the more serious the fading. The evaluation results are shown in Table 1 below.
[0108] Table 1 - Performance test results of fiber sheets prepared in the present application examples and comparative examples
[0109]
[0110] As shown in Table 1, in Example 1 of the present application, a modified pigment is added to the fiber sheet, and the modified pigment is wrapped with polyarylsulfone to form a heat-resistant layer. Polyarylsulfone itself has high temperature resistance and transparency, and will not block the organic pigment. At the same time, it can improve the high temperature resistance of the organic pigment. After high-temperature heat treatment, the crystallinity and orientation of the polyarylsulfone heat-resistant layer can be maximized, and its high temperature resistance and rigidity can be further enhanced, and the heat and pressure resistance of the pigment can be improved. Finally, the heat-resistant layer introduces polar substituent groups by combining hydroxyethyl acrylate, which can improve the solvent resistance of the modified pigment and avoid the heat-resistant layer from dissolving and rupturing in the solvent due to the long-term high temperature of the spinning process. The degree of degradation of the modified pigment after long-term high-temperature spinning treatment is low, and its light resistance, friction resistance and soap washing color fastness can reach level 4 or above.
[0111] Untreated organic pigments are added to the fiber flakes of Comparative Example 4. The organic pigments need to be in a high temperature and high pressure environment for a long time during the spinning process, which makes the organic pigments easily affected by solvents and temperature and deteriorates. The fiber flakes are prone to severe fading or discoloration after soaping or light exposure. The color fastness to soaping and light exposure are both below level 2, and the color is unstable.
[0112] The pigment added to the fiber flakes of Comparative Example 5 was not modified after being wrapped with polyarylsulfone to form a heat-resistant layer, and no polar substituent groups were introduced on the surface of the pigment, which resulted in the heat-resistant layer being easily corroded by the solvent and cracked in a high-temperature environment for a long time. The solvent caused the internal organic pigment to be exposed to a high-temperature and high-pressure environment, which easily led to deterioration. The prepared fiber flakes had poor resistance to soap washing and light exposure, and were easily faded or discolored after soap washing and light exposure.
[0113] By comparing the performance test results of Examples 1, 5-6 and Comparative Example 2 in Table 1, it can be seen that the present application controls the mass ratio of high-density polyethylene and pigment in the spinning solution of Examples 1 and 5-6 to be between (10-32): 1, which can ensure that the prepared fiber products have high strength and toughness, the nail rod tear strength of the fiber sheet can reach more than 260N / 50mm, and the tensile strength can reach more than 46N / cm, and the fiber sheet has high resistance to friction, soaping and light, and the color fastness reaches more than level 4, which can meet the application performance requirements.
[0114] The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above description is only a specific embodiment of the present application and is not intended to limit the scope of protection of the present application. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of protection of the present application.
Claims
1. A method for preparing flash-spun fibers containing organic pigments, characterized in that: The following steps are involved: The polyarylsulfone is heated and dissolved in solvent A, and then an organic pigment and a dispersant are added to obtain a mixed solution A, wherein the particle size of the organic pigment is greater than or equal to 300 nm and less than or equal to 500 nm, the mixture is homogenized and stirred, and the coated pigment is obtained after filtering. The wrapped pigment is heat-treated to isolate oxygen, the heat treatment temperature is greater than or equal to 150° C. and less than or equal to 180° C., and cooled to obtain a treated pigment. The treated pigment is placed in a solvent B containing hydroxyethyl acrylate, and then 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate is added to obtain a mixed solution B. After stirring for reaction, the solution is filtered and dried to obtain a modified pigment. The polymer melt and the modified pigment are mixed to form a uniform polymer mixture, the spinning solvent is mixed to form a uniform solvent mixture, the polymer mixture and the solvent mixture are mixed in a mixing device, heated and nitrogen is introduced to make the temperature in the mixing device greater than or equal to 200° C. and less than or equal to 220° C., and the pressure greater than or equal to 10 MPa and less than or equal to 13 MPa, and the mixture is stirred in a closed manner. After the temperature and pressure are stabilized, a spinning solution is obtained. The spinning solution is ejected through the spinneret of the connected flash spinning device, stretched and opened by an air amplifier to form an ultrafine fiber web, and then laid on a mobile device, and subjected to cold pressing and hot rolling to obtain a fiber sheet. The spinning solution comprises 16wt%-20wt% of the polymer melt, 0.5wt%-1.5wt% of the modified pigment, 0wt%-5wt% of the additive, and the balance of the spinning solvent.
2. The method for preparing a flash-spun fiber containing an organic pigment according to claim 1, wherein: The mixed solution A includes 4wt%-7wt% of the polyarylsulfone, 10wt%-18wt% of the organic pigment, 1wt%-2wt% of the dispersant and the balance of the solvent A.
3. The method for preparing a flash-spun fiber containing an organic pigment according to claim 1, wherein: The mixed solution B includes 15wt%-20wt% of the treated pigment, 3wt%-8wt% of the hydroxyethyl acrylate, 1wt%-3wt% of the 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate and the balance of the solvent B.
4. The method for preparing a flash-spun fiber containing an organic pigment according to claim 1, wherein: The mass ratio of the polymer melt to the modified pigment is (16-32):
1.
5. The method for preparing a flash-spun fiber containing an organic pigment according to claim 1, wherein: Satisfy at least one of the following a)-e): a) the mixed solution A is homogenized and stirred at a rate greater than or equal to 600 rpm and less than or equal to 800 rpm, b) the time for the heat treatment of the packaged pigment is greater than or equal to 20 minutes and less than or equal to 30 minutes, c) the reaction time of the mixed solution B is greater than or equal to 1 hour and less than or equal to 3 hours, d) the mixing equipment is sealed and stirred for a time of greater than or equal to 2 hours and less than or equal to 3 hours, e) The air flow rate ejected from the spinneret of the flash spinning equipment is greater than or equal to 10,000 m / min and less than or equal to 13,000 m / min, and the pore size of the spinneret is greater than or equal to 1 μm and less than or equal to 5 μm.
6. The method for preparing flash-spun fibers containing organic pigments according to claim 1, wherein: The organic pigment is at least one of phthalocyanine red, phthalocyanine blue, phthalocyanine green, permanent yellow, permanent violet and azo red.
7. The method for preparing a flash-spun fiber containing an organic pigment according to claim 1, wherein: The polymer melt is at least one of polyesters such as polyethylene, high-density polyethylene, polypropylene, polybutene, polymethylpentene, polyvinylidene fluoride, ethylene-tetrafluoroethylene copolymer, PET, and polylactic acid.
8. The method for preparing flash-spun fibers containing organic pigments according to claim 1, wherein: Satisfy at least one of the following a)-d): a) the solvent A is at least one of dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone, b) the dispersant is at least one of sodium dodecylbenzenesulfonate, polyvinyl alcohol, pyrrolidone, and sodium methylene dinaphthalenesulfonate, c) the solvent B is an aliphatic hydrocarbon solvent, d) The spinning solvent is at least one of toluene, benzene, n-hexane, butane, pentene, heptane, octane, cyclohexane, cyclopentane, dichloromethane, carbon tetrachloride, chloroform, chloromethane, ethyl chloride, dichloroethylene, trichlorofluoromethane, dichlorotrifluoroethane, pentafluoropropane, heptafluoropropane, perfluorohexane, perfluorohexane, perfluoroheptane, octafluorocyclopentane, and alcohol solvents.
9. Flash-spun fibers containing organic pigments prepared by the method for preparing flash-spun fibers containing organic pigments according to any one of claims 1 to 8.
10. Use of the flash-spun fiber containing organic pigments as claimed in claim 9 in the preparation of cultural and creative printed products, clothing or household products.
Citation Information
Cited By
Polyester flash non-woven fabric and preparation method thereof
CN119465518A
A kind of polyester flash nonwoven fabric and preparation method thereof
CN119465518B