Dry-type electrode and preparation method thereof, battery and electric device

By treating polytetrafluoroethylene with sodium naphthalene solution, polar groups are introduced to form a modified binder, the problem of poor bonding performance in dry electrodes is solved, and the cycle stability and capacity performance of the battery are improved.

CN118919641APending Publication Date: 2024-11-08CHINA FAW CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411073739.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The reaction of polytetrafluoroethylene with lithium ions in the dry electrode leads to a decrease in battery capacity performance and poor bonding performance, which leads to the easy fall of active substances, which increases internal resistance and affects circulation stability.

Method used

Polytetrafluoroethylene is treated with sodium naphthalene solution, and polar groups such as -OH, C=O, -COOH, C=C are introduced. Polytetrafluoroethylene is modified as a binder to enhance its active substances and conductivity. The adhesive properties of the agent form a fibrotic self-supporting electrode film.

Benefits of technology

It improves the cycle stability of the dry electrode and the battery, enhances the bonding performance, reduces the fall of active substances, and improves the cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919641A_ABST
    Figure CN118919641A_ABST
Patent Text Reader

Abstract

The invention relates to a dry electrode and a preparation method thereof, a battery and an electric device. The dry electrode comprises a self-supporting electrode film, the self-supporting electrode film comprises an active substance, a conductive agent and a binder, and the binder comprises modified polytetrafluoroethylene obtained after polytetrafluoroethylene is treated with a sodium naphthalene solution. According to the dry-type electrode, the stability of the self-supporting electrode film is improved, so that the cycling stability of the dry-type electrode and the battery provided with the dry-type electrode is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a dry electrode and a preparation method thereof, a battery and an electrical device. Background Art

[0002] With the development of electric vehicles, industrial production has higher and higher requirements for energy storage systems such as lithium-ion batteries. Dry electrodes are an emerging electrode manufacturing technology that can effectively simplify the preparation process and improve battery performance compared to wet processes. Dry electrodes are an emerging electrode manufacturing technology that can effectively simplify the preparation process and improve battery performance. Among them, polymer fibrillation is a special dry electrode manufacturing technology that uses a fibrillated binder to fiberize into a mesh structure under external force to encapsulate active substances and conductive agents. Polytetrafluoroethylene (PTFE), known as the "king of plastics", has excellent chemical resistance, thermal stability, dielectric properties, non-stickiness and wear resistance, and is a very important special engineering plastic. At the same time, PTFE has poor bonding properties with other materials, resulting in the problem that active substances are easy to fall off when used in dry electrodes, resulting in increased internal resistance of the battery. At the same time, PTFE will react with lithium ions, affecting the capacity performance of the battery. Therefore, how to improve the cycle stability of dry electrodes and batteries equipped with them is a technical problem that needs to be solved urgently. Summary of the invention

[0003] Based on this, it is necessary to provide a dry electrode with high cycle stability and a preparation method thereof, a battery and an electrical device.

[0004] The present application is implemented through the following technical solutions.

[0005] In one aspect of the present application, a dry electrode is provided, comprising a self-supporting electrode membrane, wherein components of the self-supporting electrode membrane include an active material, a conductive agent and a binder, wherein the binder includes modified polytetrafluoroethylene obtained by treating polytetrafluoroethylene with a sodium naphthalene solution.

[0006] In some of the embodiments, at least one of the following conditions is met:

[0007] (1) The thickness of the self-supporting electrode film is 100 μm to 150 μm;

[0008] (2) The mass volume ratio of the polytetrafluoroethylene to the sodium naphthalene solution is 1 g: (2-4) mL;

[0009] (3) The modified polytetrafluoroethylene has a carbonized layer with a thickness of 0.05 μm to 1 μm on its surface;

[0010] (4) The dry electrode further comprises a current collector, and the self-supporting electrode film is disposed on at least one side of the current collector.

[0011] In some embodiments, the sodium naphthalene solution includes naphthalene, metallic sodium, and a diluent, and the diluent includes at least one of tetrahydrofuran and toluene.

[0012] In some of the embodiments, the sodium naphthalene solution is prepared by mixing the sodium naphthalene treatment solution and the diluent in a volume ratio of 1: (1-2).

[0013] In some of the embodiments, at least one of the following conditions is met:

[0014] (1) The conductive agent includes at least one of Super P, CNTs and conductive graphite;

[0015] (2) In the self-supporting electrode film, the mass content of the active material is 50% to 96%;

[0016] (3) In the self-supporting electrode film, the mass content of the conductive agent is 2% to 40%;

[0017] (4) In the self-supporting electrode film, the mass content of the binder is 2% to 10%.

[0018] In some embodiments, the active material is a positive electrode active material, and the positive electrode active material includes at least one of lithium manganese nickel oxide, lithium iron phosphate, lithium cobalt oxide and a ternary material; or,

[0019] The active material is a negative electrode active material, and the negative electrode active material includes at least one of graphite, activated carbon, hard carbon material, soft carbon material, silicon-based negative electrode material and lithium titanate.

[0020] In some of the embodiments, the active material is a positive electrode active material, and the binder further comprises a positive electrode fluorine-based polymer; or,

[0021] The active material is a negative electrode active material, and the binder further comprises at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer, sodium carboxymethyl cellulose and styrene-butadiene rubber.

[0022] In some of the embodiments, at least one of the following conditions is met:

[0023] (1) The positive electrode fluorine-based polymer includes at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer and polyvinylidene fluoride;

[0024] (2) The elongation of the positive electrode fluorine-based polymer is 220% to 500%;

[0025] (3) The compression ratio of the positive electrode fluorine-based polymer is 300-4000;

[0026] (4) The melting point of the positive electrode fluorine-based polymer is 220~380℃.

[0027] In another aspect of the present application, a method for preparing the above-mentioned dry electrode is provided, comprising the following steps:

[0028] The active material, the conductive agent and the binder containing the modified polytetrafluoroethylene are dispersed to form a mixture, and the mixture is fiberized and then rolled to form the self-supporting electrode film.

[0029] In another aspect of the present application, a battery is provided, comprising a positive electrode sheet and a negative electrode sheet arranged opposite to each other, wherein at least one of the positive electrode sheet and the negative electrode sheet is a dry electrode as described above.

[0030] In another aspect of the present application, there is provided an electrical device comprising the above-mentioned battery.

[0031] The binder used in the self-supporting electrode film of the above-mentioned dry electrode includes modified polytetrafluoroethylene treated with sodium naphthalene solution. The modified polytetrafluoroethylene introduces polar groups such as -OH, C=O, -COOH, C=C on the surface after being treated with sodium naphthalene treatment solution, so that the surface energy of the modified polytetrafluoroethylene is increased, the contact angle is reduced, and the wettability is improved, thereby improving the shortcomings of polytetrafluoroethylene such as large contact angle, small surface tension, and poor surface wetting performance, and improving its bonding performance with active substances and conductive agents, thereby improving the stability of the self-supporting electrode film, and then improving the cycle stability of the dry electrode and the battery provided with it.

[0032] The preparation method of the above dry electrode is simple, and the modified PTFE can be fibrous under the action of shear force. When applied to the binder of the electrode in lithium-ion batteries and other batteries, the active material and the conductive additive can be connected and coated together to improve the structural stability of the dry electrode during the cycle operation. In the above dry electrode, the modified PTFE is a fibrous modified PTFE. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the infrared spectrum of the modified polytetrafluoroethylene prepared in Example 1 of the present application;

[0034] Figure 2 This is a scanning electron microscope image of the self-supporting electrode film in the positive electrode sheet prepared in Example 3 of the present application.

[0035] Figure 3 This is a test chart of the cycle performance of the half-cell assembled with the positive electrode sheet prepared in Example 3 of the present application. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0038] "Scope" disclosed in the present application can be limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or excluding end values, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 listed, and if the maximum range values ​​3,4 and 5 are also listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0039] In the description of the present invention, “plurality” means two or more than two, unless otherwise clearly and specifically defined.

[0040] In one aspect of the present application, a dry electrode and a preparation method thereof are provided. The dry-process battery will be introduced in detail below in conjunction with the preparation method.

[0041] The dry electrode provided in one embodiment of the present application includes a self-supporting electrode film. The components of the self-supporting electrode film include active materials, conductive agents and binders, and the binder includes modified polytetrafluoroethylene treated with sodium naphthalene solution.

[0042] Another embodiment of the present application provides a method for preparing the above-mentioned dry electrode, comprising the following steps: dispersing the active material, the conductive agent and the binder containing modified polytetrafluoroethylene to form a mixture, and fiberizing the mixture and then forming a self-supporting electrode film under rolling action.

[0043] The binder used in the self-supporting electrode film of the above-mentioned dry electrode includes modified polytetrafluoroethylene treated with sodium naphthalene solution. The modified polytetrafluoroethylene introduces polar groups such as -OH, C=O, -COOH, C=C on the surface after being treated with sodium naphthalene treatment solution, so that the surface energy of the modified polytetrafluoroethylene is increased, the contact angle is reduced, and the wettability is improved, thereby improving the shortcomings of polytetrafluoroethylene such as large contact angle, small surface tension, and poor surface wetting performance, and improving its bonding performance with active substances and conductive agents, thereby improving the stability of the self-supporting electrode film, and then improving the cycle stability of the dry electrode and the battery provided with it.

[0044] The preparation method of the above dry electrode is simple, and the modified PTFE can be fibrous under the action of shear force. When applied to the binder of the electrode in lithium-ion batteries and other batteries, the active material and the conductive additive can be connected and coated together to improve the structural stability of the dry electrode during the cycle operation. In the above dry electrode, the modified PTFE is a fibrous modified PTFE.

[0045] The modified PTFE can be used to prepare a positive electrode sheet or a negative electrode sheet. That is, the dry electrode can be a positive electrode sheet or a negative electrode sheet.

[0046] In some of the embodiments, the thickness of the self-supporting electrode film is 100 μm to 150 μm. As an example, the thickness can be 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, or can be in a range consisting of any two of the above point values ​​as end values, such as 120 μm to 150 μm, and similarly below. The thickness of the self-supporting electrode film within this range can further improve the cycle performance of the battery.

[0047] In some of the embodiments, the mass volume ratio of polytetrafluoroethylene to sodium naphthalene solution is 1g: (2-4) mL, for example, 1g: 2mL, 1g: 3mL, 1g: 4mL. Controlling this mass volume ratio can further improve the bonding performance of the prepared modified PTFE, thereby improving the stability of the electrode and the cycle stability of the battery.

[0048] In some embodiments, the sodium naphthalene solution includes naphthalene, metallic sodium and a diluent, and the diluent includes at least one of tetrahydrofuran and toluene. Further, the sodium naphthalene solution is prepared by mixing a sodium naphthalene treatment solution and a diluent in a volume ratio of 1: (1-2). As an example, the volume ratio may be 1: 1, 1: 1.5, or 1: 2. Further, the sodium naphthalene treatment solution includes naphthalene and metallic sodium. Further, the mass ratio of metallic sodium to naphthalene in the sodium naphthalene treatment solution is 1: (1-10), and the mass ratio may be 1: 1, 1: 2, 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8, 1: 9, or 1: 10. Further, the diluent is tetrahydrofuran.

[0049] Furthermore, the step of treating polytetrafluoroethylene with sodium naphthalene solution to obtain modified polytetrafluoroethylene includes: mixing polytetrafluoroethylene with sodium naphthalene solution and stirring for 2 minutes to 60 minutes, then filtering, washing the solid with tetrahydrofuran, water and acetone in sequence, filtering the solid, and drying it by vacuum or other methods to obtain modified PTFE particles.

[0050] Furthermore, the temperature for fiberizing the mixture may be 20° C. to 25° C.; after fiberizing and before rolling, the process may further include a step of converting the mixture into a flocculent or soft mass-like mixture under the action of shear force.

[0051] Furthermore, the step of fiberizing the mixture and then forming a self-supporting electrode film under roller pressure can be performed in a fibrillation film-making machine. The fiberization step can also be performed by manual or mechanical grinding fiberization.

[0052] In some embodiments, the surface of the modified polytetrafluoroethylene has a carbonized layer with a thickness of 0.05 μm to 1 μm. The carbonized layer is brown. As an example, the thickness of the carbonized layer can be 0.05 μm, 0.1 μm, 0.2 μm, 0.5 μm, or 1 μm.

[0053] In some embodiments, the dry electrode further comprises a current collector, and the self-supporting electrode film is disposed on at least one side of the current collector. Further, the self-supporting electrode film can be disposed on one side or both sides of the current collector by hot pressing.

[0054] In one example, the dry electrode is a positive electrode sheet, and the current collector can be a metal foil or a composite current collector. For example, aluminum foil can be used as the metal foil. The composite current collector can include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer, the same below.

[0055] In some of the embodiments, the dry electrode is a positive electrode sheet, and the active material in the dry electrode is a positive electrode active material, which includes but is not limited to lithium manganese nickel oxide, lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2) and at least one of the ternary materials.

[0056] Further, the ternary material includes but is not limited to at least one of a nickel-cobalt-manganese ternary material (NCM) and a nickel-cobalt-aluminum ternary material (NCA). As an example, the nickel-cobalt-manganese ternary material (NCM) includes but is not limited to LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2. Nickel-cobalt-aluminum ternary materials (NCA) may include LiNi 0.8 Co 0.15 Al 0.05 O2.

[0057] In some embodiments, the dry electrode is a positive electrode sheet, and the active material in the dry electrode is a positive electrode active material. The binder also includes a positive electrode fluorine-based polymer. Further, in the binder, the mass content of the positive electrode fluorine-based polymer is 0-50%, for example, 0, 1%, 2%, 3%, 5%, 10%, 20%, 30%, 40%, 50%.

[0058] It is understood that in some examples, the binder is the modified PTFE mentioned above.

[0059] Furthermore, the positive electrode fluorine-based polymer includes at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer and polyvinylidene fluoride.

[0060] Furthermore, the elongation of the positive electrode fluorine-based polymer is 220% to 500%, and as an example, it can be 220%, 250%, 300%, 400% or 500%. A larger elongation means that the polymer has better mechanical properties, which is beneficial to the structural stability of the electrode during the cycle.

[0061] Further, the compression ratio of the positive electrode fluorine-based polymer is 300-4000, and as an example, it can be: 300, 500, 1000, 2000, 3000 or 4000. A larger compression ratio is beneficial to the processing of the binder in the battery system.

[0062] Further, the melting point of the positive electrode fluorine-based polymer is 220-380° C., and as an example, it can be: 220° C., 250° C., 280° C., 300° C., 350° C. or 380° C. Good thermal stability is conducive to the binder to maintain its own stability when the internal ambient temperature of the electrode increases.

[0063] In one example, the dry electrode is a negative electrode sheet, and the current collector can be a metal foil or a composite current collector. As the metal foil, copper foil can be used.

[0064] In some of the embodiments, the dry electrode is a negative electrode sheet, and the active material in the dry electrode is a negative electrode active material, which includes at least one of graphite, activated carbon, hard carbon material, soft carbon material, silicon-based negative electrode material and lithium titanate.

[0065] In some of the embodiments, the dry electrode is a negative electrode sheet, the active material is a negative electrode active material, and the binder also includes at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer, sodium carboxymethyl cellulose and styrene-butadiene rubber.

[0066] In some embodiments, the conductive agent includes but is not limited to at least one of Super P, CNTs and conductive graphite.

[0067] In some of the embodiments, in the self-supporting electrode film, the mass content of the active material is 50% to 96%, and as examples may be 50%, 60%, 70%, 80%, 85%, 90%, 92%, 95%, 96%.

[0068] In some of the embodiments, in the self-supporting electrode film, the mass content of the conductive agent is 2% to 40%, and as examples may be 2%, 4%, 5%, 6%, 8%, 10%, 20%, 30%, 40%.

[0069] In some embodiments, in the self-supporting electrode film, the mass content of the binder is 2% to 10%, and may be 2%, 4%, 5%, 6%, 8%, or 10% as examples.

[0070] In another aspect of the present application, a battery is provided, comprising a positive electrode sheet and a negative electrode sheet arranged opposite to each other, wherein at least one of the positive electrode sheet and the negative electrode sheet is a dry electrode as described above.

[0071] In the above-mentioned battery, at least one of the positive electrode sheet and the negative electrode sheet is a dry electrode as described above, so that the stability of the electrode is improved, thereby improving the cycle stability of the battery.

[0072] The battery also includes an electrolyte that is soaked in the positive electrode sheet and the negative electrode sheet. The electrolyte includes an electrolyte salt and a solvent. The electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0073] In some of the embodiments, the solvent may include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate, fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0074] The battery also includes a separator, which is disposed between the positive electrode and the negative electrode, and mainly prevents the positive and negative electrodes from short-circuiting, while allowing ions to pass through. In some embodiments, the material of the separator may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.

[0075] The above-mentioned battery can be, but is not limited to, a lithium ion battery, a lithium metal battery, or a sodium ion battery.

[0076] In another aspect of the present application, there is provided an electrical device comprising the above-mentioned battery.

[0077] The electrical devices may include, but are not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, the mobile devices may be, for example, mobile phones, laptop computers, etc.; the electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to these.

[0078] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0079] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments.

[0080] Example 1: Preparation of polytetrafluoroethylene treated with sodium naphthalene solution

[0081] Take about 10g PTFE in a beaker, add 10mL FS-004 sodium naphthalene treatment solution, add 10mL tetrahydrofuran solution for dilution, keep the volume ratio of sodium naphthalene treatment solution to tetrahydrofuran at 1:1 to treat PTFE. Start stirring for about 2-4 minutes, after the surface of PTFE turns into a brown carbonized layer, continue stirring for 10-30 minutes. Repeat the above operation until the required amount of PTFE is obtained, pour into the sieve, rinse three times with tetrahydrofuran, water and acetone respectively, let stand and filter for 2 hours, vacuum dry for 8 hours, and obtain modified polytetrafluoroethylene particles.

[0082] Example 2: Preparation of polytetrafluoroethylene treated with sodium naphthalene solution

[0083] Take about 5g PTFE in a beaker, add 10mL FS-004 sodium naphthalene treatment solution, add 10mL tetrahydrofuran solution for dilution, keep the volume ratio of sodium naphthalene treatment solution to tetrahydrofuran at 1:1 to treat PTFE. Start stirring for about 2-4min, after the surface of PTFE turns into a brown carbonized layer, continue stirring for 10-30 minutes. Repeat the above operation until the required amount of PTFE is obtained, pour into the sieve, rinse three times with tetrahydrofuran, water and acetone respectively, let stand and filter for 2h, vacuum dry for 8h, and obtain modified polytetrafluoroethylene particles.

[0084] Example 3: Battery Preparation

[0085] With a mass fraction of 95% LiNi 0.8 Co 0.1 Mn 0.1O2 was used as the active material, mixed with 3% of the conductive agent Super P at room temperature for 1 hour, and 2% of the modified polytetrafluoroethylene particles prepared in Example 1 were added and mixed at -10°C for 2 hours to prepare a multi-component mixture of binders without deformation, ground and fiberized at 20°C, and then mixed for 20 minutes to prepare a granular coating; the obtained granular coating was rolled at 100°C into a continuous positive self-supporting electrode film with a thickness of 150μm. The positive self-supporting electrode film was then hot-pressed and attached to the positive current collector aluminum foil to prepare a positive electrode sheet.

[0086] DEC (diethyl carbonate) and EC (ethylene carbonate) in a volume ratio of 1:1 were used as solvents, and LiPF6 was added to prepare a 1 mol / L LiPF6 electrolyte. The battery was assembled using Celgard 2500 as a separator and a metal Li sheet as a negative electrode.

[0087] Example 4: Battery Preparation

[0088] With a mass fraction of 95% LiNi 0.6 Co 0.2 Mn 0.2 O2 was used as the active material, mixed with 3% of the conductive agent Super P at room temperature for 1 hour, and 2% of the modified polytetrafluoroethylene particles prepared in Example 1 were added and mixed at -10°C for 2 hours to prepare a multi-component mixture of binders without deformation, ground and fiberized at 20°C, and then mixed for 20 minutes to prepare a granular coating; the obtained granular coating was rolled at 100°C into a continuous positive self-supporting electrode film with a thickness of 150μm. The positive self-supporting electrode film was then hot-pressed and attached to the positive current collector aluminum foil to prepare a positive electrode sheet.

[0089] DEC (diethyl carbonate) and EC (ethylene carbonate) in a volume ratio of 1:1 were used as solvents, and LiPF6 was added to prepare a 1 mol / L LiPF6 electrolyte. The battery was assembled using Celgard 2500 as a separator and a metal Li sheet as a negative electrode.

[0090] Example 5: Battery Preparation

[0091] 95% by mass of LiFePO4 was used as the active material, and 3% by mass of the conductive agent Super P was mixed at room temperature for 1 hour, and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1 were added and mixed at -10°C for 2 hours to prepare a multi-component mixture of binders without deformation, which was ground and fiberized at 20°C, and then mixed for 20 minutes to prepare a granular coating; the obtained granular coating was rolled at 100°C into a continuous positive self-supporting electrode film with a thickness of 120 μm. The positive self-supporting electrode film was then hot-pressed and attached to the positive current collector aluminum foil to prepare a positive electrode sheet.

[0092] DEC (diethyl carbonate) and EC (ethylene carbonate) in a volume ratio of 1:1 were used as solvents, and LiPF6 was added to prepare a 1 mol / L LiPF6 electrolyte. The battery was assembled using Celgard 2500 as a separator and a metal Li sheet as a negative electrode.

[0093] Example 6: Battery Preparation

[0094] 95% of LiCoO2 was used as the active material, and 3% of the conductive agent Super P was mixed at room temperature for 1 hour, and 2% of the modified polytetrafluoroethylene particles prepared in Example 1 were added and mixed at -10°C for 2 hours to prepare a multi-component mixture of binders without deformation, which was ground and fiberized at 20°C, and then mixed for 20 minutes to prepare a granular coating; the obtained granular coating was rolled at 100°C into a continuous positive self-supporting electrode film with a thickness of 120 μm. The positive self-supporting electrode film was then hot-pressed and attached to the positive current collector aluminum foil to prepare a positive electrode sheet.

[0095] DEC (diethyl carbonate) and EC (ethylene carbonate) in a volume ratio of 1:1 were used as solvents, and LiPF6 was added to prepare a 1 mol / L LiPF6 electrolyte. The battery was assembled using Celgard 2500 as a separator and a metal Li sheet as a negative electrode.

[0096] Example 7: Battery Preparation

[0097] It is basically the same as Example 3, except that the conductive agent is replaced by conductive agent CNTs of equal mass.

[0098] Example 8: Battery Preparation

[0099] It is basically the same as Example 4, except that the conductive agent is replaced by conductive agent CNTs of equal mass.

[0100] Example 9: Battery Preparation

[0101] It is basically the same as Example 5, except that the conductive agent is replaced by conductive agent CNTs of equal mass.

[0102] Example 10: Battery Preparation

[0103] It is basically the same as Example 6, except that the conductive agent is replaced by conductive agent CNTs of equal mass.

[0104] Example 11: Battery Preparation

[0105] The same as Example 7, except that the formula of the positive electrode self-supporting film is different, specifically, LiNi with a mass fraction of 96% 0.8 Co 0.1 Mn 0.1O2 is used as the active material, 2% by mass of the conductive agent Super P and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0106] Example 12: Battery Preparation

[0107] The same as Example 8, except that the formula of the positive electrode self-supporting film is different, specifically, LiNi with a mass fraction of 96% 0.6 Co 0.2 Mn 0.2 O2 is used as the active material, 2% by mass of the conductive agent Super P and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0108] Example 13: Battery Preparation

[0109] It is basically the same as Example 5, except that the formula of the positive electrode self-supporting film is different, specifically, 96% by mass of LiFePO4 as the active material, 2% by mass of the conductive agent Super P, and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0110] Example 14: Battery Preparation

[0111] It is basically the same as Example 6, except that the formula of the positive electrode self-supporting film is different, specifically, 96% by mass of LiCoO2 as the active material, 2% by mass of the conductive agent Super P, and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0112] Example 15: Battery Preparation

[0113] The same as Example 7, except that the formula of the positive electrode self-supporting film is different, specifically, LiNi with a mass fraction of 96% 0.8 Co 0.1 Mn 0.1 O2 is used as the active material, 2% by mass of the conductive agent CNTs and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0114] Example 16: Battery Preparation

[0115] The same as Example 8, except that the formula of the positive electrode self-supporting film is different, specifically, LiNi with a mass fraction of 96% 0.6 Co 0.2 Mn 0.2 O2 is used as the active material, 2% by mass of the conductive agent CNTs and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0116] Example 17: Battery Preparation

[0117] It is basically the same as Example 5, except that the formula of the positive electrode self-supporting film is different, specifically, 96% by mass of LiFePO4 as the active material, 2% by mass of the conductive agent CNTs, and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0118] Example 18: Battery Preparation

[0119] It is basically the same as Example 6, except that the formula of the positive electrode self-supporting film is different, specifically, 96% by mass of LiCoO2 as the active material, 2% by mass of the conductive agent CNTs, and 2% by mass of the modified polytetrafluoroethylene particles prepared in Example 1.

[0120] Example 19: Battery Preparation

[0121] The same as Example 3, except that the formula of the positive electrode self-supporting film is different, specifically: LiNi with a mass fraction of 90% 0.8 Co 0.1 Mn 0.1 A dry-process positive electrode sheet was prepared using O2 as the active material, 5% by mass of the conductive agent Super P, and 5% by mass of the modified polytetrafluoroethylene particles obtained in Example 1 as a binder, and a half-cell was assembled with a lithium sheet as the counter electrode for testing.

[0122] Example 20: Battery Preparation

[0123] The same as Example 3, except that the formula of the positive electrode self-supporting film is different, specifically: LiNi with a mass fraction of 85% 0.8 Co 0.1 Mn 0.1 A dry-process positive electrode sheet was prepared using O2 as the active material, 7% by mass of the conductive agent Super P, and 8% by mass of the modified polytetrafluoroethylene particles obtained in Example 1 as a binder, and a half-cell was assembled with a lithium sheet as the counter electrode for testing.

[0124] Comparative Example 1

[0125] The method is basically the same as Example 3, except that the modified polytetrafluoroethylene particles prepared in Example 1 are replaced by modified polytetrafluoroethylene particles treated with toluene of equal mass.

[0126] The preparation steps of modified polytetrafluoroethylene particles treated with toluene are as follows:

[0127] Take about 10g of PTFE in a beaker, add 10mL of toluene, and add 10mL of tetrahydrofuran solution to dilute the PTFE. Start stirring for about 2-4 minutes, and after the surface of the PTFE turns into a brown carbonized layer, continue stirring for 10-30 minutes. Repeat the above operation until the required amount of PTFE is obtained, pour it into the sieve, rinse it three times with tetrahydrofuran, water and acetone respectively, let it stand and filter for 2 hours, and vacuum dry it for 8 hours to obtain modified polytetrafluoroethylene particles.

[0128] The following is a performance test.

[0129] (I) The modified polytetrafluoroethylene obtained in Example 1 was subjected to infrared detection and analysis, and the infrared spectrum obtained was as follows: Figure 1 As shown. Among them, 1425cm -1 The absorption peak at 1639cm -1 The absorption peak at 3650cm corresponds to the stretching vibration of C=C. -1 -3610cm -1 The range corresponds to the absorption peak of free -OH. This proves that polar groups such as -OH and C=C are introduced into the surface of modified polytetrafluoroethylene. The surface energy of modified polytetrafluoroethylene is increased, the contact angle is reduced, the wettability is improved, and the difficult-to-bond polytetrafluoroethylene is improved into a bondable plastic.

[0130] (ii) The morphology of the self-supporting electrode film in the positive electrode sheet prepared in Example 3 was analyzed, and the obtained scanning electron microscope image was as follows: Figure 2 As shown in the figure, obvious filaments can be seen, which are formed by PTFE under the action of shear force, proving that the modified PTFE can normally produce fibrosis behavior.

[0131] (III) Cyclic performance tests were performed on the above-mentioned Examples 3 to 6, Examples 19 to 20 and Comparative Example 1. The specific conditions of the cyclic performance tests were as follows: using a Xinwei battery testing system with a test voltage range of 3-4.2V; performing the cyclic performance test at a current of 0.1C, and the time recording condition was 30s.

[0132] The test results of Example 3 are as follows Figure 3 As shown, the first discharge specific capacity is 190.88 mAh / g, the discharge specific capacity after 100 cycles is 146.49 mAh / g, and the capacity retention rate is 76.7%, showing excellent cycle performance.

[0133] The capacity retention rate after 100 cycles = capacity after 100 cycles / capacity after the first cycle.

[0134] The results are shown in Table 1 below.

[0135] Table 1

[0136]

[0137] It can be seen from the above table that the battery prepared in the examples of the present application has a higher cycle stability.

[0138] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0139] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.

Claims

1. A dry electrode, characterized in that: The invention comprises a self-supporting electrode film, the components of which include active material, conductive agent and adhesive, and the adhesive comprises modified polytetrafluoroethylene which is obtained by treating polytetrafluoroethylene with sodium naphthalene solution.

2. The dry electrode according to claim 1, characterized in that At least one of the following conditions is met: (1) The thickness of the self-supporting electrode film is 100 μm to 150 μm; (2) The mass volume ratio of the polytetrafluoroethylene to the sodium naphthalene solution is 1 g: (2-4) mL; (3) The modified polytetrafluoroethylene has a carbonized layer with a thickness of 0.05 μm to 1 μm on its surface; (4) The dry electrode further comprises a current collector, and the self-supporting electrode film is disposed on at least one side of the current collector.

3. The dry electrode according to claim 1, characterized in that The sodium naphthalene solution comprises naphthalene, metallic sodium and a diluent, and the diluent comprises at least one of tetrahydrofuran and toluene.

4. The dry electrode according to claim 3, characterized in that The sodium naphthalene solution is prepared by mixing the sodium naphthalene treatment solution and the diluent in a volume ratio of 1: (1-2).

5. The dry electrode according to claim 1, characterized in that At least one of the following conditions is met: (1) The conductive agent includes at least one of Super P, CNTs and conductive graphite; (2) In the self-supporting electrode film, the mass content of the active material is 50% to 96%; (3) In the self-supporting electrode film, the mass content of the conductive agent is 2% to 40%; (4) In the self-supporting electrode film, the mass content of the binder is 2% to 10%.

6. The dry electrode according to claim 1, characterized in that The active material is a positive electrode active material, and the positive electrode active material includes at least one of lithium manganese nickel oxide, lithium iron phosphate, lithium cobalt oxide and a ternary material; or, The active material is a negative electrode active material, and the negative electrode active material includes at least one of graphite, activated carbon, hard carbon material, soft carbon material, silicon-based negative electrode material and lithium titanate.

7. The dry electrode according to any one of claims 1 to 6, characterized in that: The active material is a positive electrode active material, and the binder further comprises a positive electrode fluorine-based polymer; or, The active material is a negative electrode active material, and the binder further comprises at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer, sodium carboxymethyl cellulose and styrene-butadiene rubber.

8. The dry electrode according to claim 7, characterized in that At least one of the following conditions is met: (1) The positive electrode fluorine-based polymer includes at least one of polyperfluoroethylene propylene, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, ethylene-tetrafluoroethylene copolymer and polyvinylidene fluoride; (2) The elongation of the positive electrode fluorine-based polymer is 220% to 500%; (3) The compression ratio of the positive electrode fluorine-based polymer is 300-4000; (4) The melting point of the positive electrode fluorine-based polymer is 220~380℃.

9. The method for preparing a dry electrode according to any one of claims 1 to 8, characterized in that: The steps include: The active material, the conductive agent and the binder containing the modified polytetrafluoroethylene are dispersed to form a mixture, and the mixture is fiberized and then rolled to form the self-supporting electrode film.

10. A battery, characterized in that: It comprises a positive electrode sheet and a negative electrode sheet which are arranged opposite to each other, and at least one of the positive electrode sheet and the negative electrode sheet is a dry electrode as claimed in any one of claims 1 to 8.

11. An electrical device, characterized in that: Comprising the battery as claimed in claim 10.

Citation Information

Cited By

  • Dry electrode and manufacturing method therefor, battery, and electric device

    WO2026031815A1