Negative plate, preparation method of negative plate, pole group and lithium ion battery

By designing an optimized coating structure on the negative electrode of the lithium-ion battery, the N/P ratio of the negative electrode to the positive electrode is improved, and lithium-ion battery is prevented, which solves the safety problems caused by insufficient lithium embedded position in the lithium battery and improves the safety performance of the battery and energy density.

CN118919653APending Publication Date: 2024-11-08TIANJIN JUYUAN NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410930169.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the charging process, lithium dendrites are grown due to insufficient lithium embedded position of the negative electrode, which causes short circuits of the positive and negative electrodes through the diaphragm, causing thermal runaway and safety problems. In order to prevent lithium excretion, excessive negative electrode materials are usually required, and the battery is lost. Capacity and energy density.

Method used

A negative electrode sheet is designed, which includes first and second coatings coated on both sides of the current collector, the amount of the winding area of ​​the first coating is greater than the plane region, and the amount of the winding area of ​​the second coating is applied to The N/P ratio of the negative electrode to the positive electrode is improved by optimizing the coating structure, preventing lithium evolution, and reducing the content of the negative electrode active material.

Benefits of technology

Effectively prevent lithium dissipation in the battery winding area, improve battery safety performance, maintain battery energy density, and avoid thermal runaway and safety problems caused by lithium dissipation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919653A_ABST
    Figure CN118919653A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of batteries, and particularly relates to a negative plate, a preparation method thereof, a pole group and a lithium ion battery. The negative plate comprises a current collector as well as a first coating and a second coating which are coated on two sides of the current collector; the first coating and the second coating respectively and independently comprise a plane area and a winding area which are arranged at an interval; according to the negative plate, the coating amount of the first winding area is greater than the coating amount of the first plane area, so that the N / P ratio of the first coating surface of the negative electrode to the positive plate can be improved, and lithium precipitation is effectively prevented. And meanwhile, the coating amount of the negative electrode second winding area is smaller than that of the negative electrode second plane area, so that the content ratio of the negative electrode active material in the battery is reduced. Therefore, the whole pole group can effectively prevent lithium precipitation in a battery winding area while the energy density of the battery is not influenced, and the safety performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to a negative electrode sheet and a preparation method thereof, an electrode group, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are now widely used in various fields of life and production, such as wearables, electronic devices, new energy vehicles, and corporate manufacturing. At the same time, the safety of lithium-ion batteries has always been a focus of attention. The safety failure of batteries is mainly caused by thermal runaway of lithium-ion batteries. The main cause of thermal runaway is battery short circuit, which causes battery fire and explosion. The main cause of battery safety failure is lithium precipitation. When the battery is charging, lithium ions migrate from the positive electrode to the negative electrode. If the negative electrode does not provide enough lithium insertion sites, lithium ions will precipitate at the negative electrode of the battery to form lithium dendrites. As the lithium dendrites grow, they will pierce the diaphragm, causing a short circuit between the positive and negative electrodes, thermal runaway of the battery, and cause safety problems.

[0003] At the corners of the wound electrode group, since the first coating of the negative electrode faces outward (relative to the second coating), it receives the migration of lithium ions in the outer positive electrode sheet. Compared with the outer positive electrode sheet, the area of ​​the negative electrode sheet in the inner circle is slightly smaller, and the lithium embedding position may not be enough, and the risk of lithium precipitation is greater. In order to prevent lithium precipitation from the negative electrode sheet, the negative electrode is generally excessive to the positive electrode, but the excess of the negative electrode is large, which will lose battery capacity and reduce battery energy density. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a negative electrode sheet and a preparation method thereof, an electrode group, and a lithium ion battery.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A negative electrode sheet comprises a current collector and a first coating and a second coating coated on both sides of the current collector; the first coating and the second coating respectively and independently comprise a plane area and a winding area which are arranged at intervals; the plane area and the winding area respectively correspond to the plane area and the winding area of ​​the negative electrode sheet wound to form a pole group; the first coating is placed outside the pole group relative to the second coating when forming the pole group; the first coating comprises a first plane area and a first winding area; the second coating comprises a second plane area and a second winding area.

[0007] Preferably, the coating length of the first coating is greater than the coating length of the negative electrode second coating;

[0008] The coating amount of the first winding area is greater than the coating amount of the first plane area.

[0009] The coating amount of the second winding area is smaller than that of the second plane area.

[0010] The coating amount of the first plane area is equal to the coating amount of the second plane area.

[0011] The coating amount of the first plane area is 10-30 mg / cm 2 , and the coating amount in the first winding area is higher than that in the first plane area by 0.7-2 mg / cm 2 .

[0012] Preferably, the coating amount of the second plane area is 10-30 mg / cm 2 , and the coating amount of the second winding area is 0.5-1.0mg / cm lower than that of the second plane area 2 .

[0013] The present invention also includes a method for preparing the negative electrode sheet, comprising the following steps: preparing negative electrode slurry; coating the negative electrode slurry on both sides of the negative electrode current collector to obtain a first coating and a second coating, and then drying, rolling and shearing to prepare the negative electrode sheet.

[0014] The negative electrode slurry comprises a negative electrode active material, a negative electrode conductive agent, a negative electrode dispersant, and a negative electrode binder;

[0015] The mass ratio of the negative electrode active material, the negative electrode conductive agent, the negative electrode dispersant, and the negative electrode binder is (90-98): (0.1-2): (0.1-4): (1-4);

[0016] Preferably, the negative electrode active material is artificial graphite; the conductive agent is one or more of conductive carbon black and carbon nanotubes;

[0017] Preferably, the negative electrode dispersant is sodium carboxymethyl cellulose.

[0018] Preferably, the negative electrode binder is styrene-butadiene rubber latex.

[0019] The present invention also includes an electrode group, including a positive electrode sheet and the negative electrode sheet, a positive electrode sheet and a separator; the first coating of the negative electrode sheet is placed outside the electrode group relative to the second coating when the electrode group is formed.

[0020] The positive electrode sheet is prepared in the following manner: positive electrode active material: positive electrode conductive agent: positive electrode binder are added into an organic solvent in a mass ratio of (90-98): (1-5): (1-5), vacuumed and mixed in a blender to disperse to prepare a positive electrode slurry, which is then coated, rolled and sheared to prepare a positive electrode sheet.

[0021] The coating amount of positive electrode active material is 15-50mg / cm 2 .

[0022] Preferably, the positive electrode active material is a lithium cobalt oxide material, a nickel-cobalt-manganese ternary material, a lithium manganate material or a lithium iron phosphate material, the positive electrode conductive agent is one or more of conductive carbon black and carbon nanotubes; the positive electrode binder is one or more of a homopolymer or copolymer of polyvinylidene fluoride;

[0023] Preferably, the drying temperature is 70°C-130°C.

[0024] The present invention also includes a lithium-ion battery, comprising the electrode group and electrolyte according to any one of claims 8 to 9; the lithium-ion battery is prepared by the following method: the positive electrode sheet, the negative electrode sheet and the separator are prepared into an electrode group by winding, and the lithium-ion battery is prepared by aluminum-plastic packaging, liquid injection, standing, pressurized formation, and degassing;

[0025] Preferably, the manufactured lithium-ion battery is subjected to a cycle test, where the battery is charged at 1C until fully charged and then rested for 10 minutes, and then discharged at 1C. After the charge and discharge are repeated 500 times, the battery is fully charged and disassembled to observe whether there is obvious lithium deposition at the negative electrode.

[0026] Preferably, the thickness of the aluminum-plastic is 110-160um, and the temperature of battery formation is 70°C-95°C; preferably, the temperature range of the injection process is 18-26°C, and the time from the start of injection to the end of injection does not exceed 12 hours; preferably, the environment for disassembling the battery requires a dew point temperature less than -34.5 degrees Celsius.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The negative electrode sheet of the present application uses the coating amount of the first winding area to be greater than the coating amount of the first plane area, which can increase the N / P ratio of the first coating layer of the negative electrode facing the positive electrode sheet and effectively prevent lithium deposition. At the same time, since the coating amount of the second winding area of ​​the negative electrode is less than the coating amount of the second plane area of ​​the negative electrode, the proportion of the negative electrode active material content in the battery is reduced. As a result, the entire electrode group can effectively prevent lithium deposition in the winding area of ​​the battery without affecting the energy density of the battery, thereby improving the safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram showing the structure of the first coating layer according to an embodiment of the present invention is shown;

[0030] Figure 2 A schematic diagram showing the structure of the negative electrode sheet of the present invention before winding;

[0031] Figure 3 A schematic diagram showing the structure of the second coating layer according to an embodiment of the present invention is shown;

[0032] Figure 4 A schematic diagram showing the structure of the present invention wound into a pole group;

[0033] Figure 5 A schematic diagram showing the structure of the winding area wound into a pole group of the present invention is shown. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.

[0035] Figure 1-3 A negative electrode sheet is shown, comprising a current collector 1 and a first coating layer and a second coating layer coated on both sides of the current collector; the first coating layer and the second coating layer independently comprise a plane area 11 and a winding area 12 ( Figure 5 ); the plane area and the winding area correspond to the plane area and the winding area of ​​the electrode group formed by winding the negative electrode sheet respectively; the first coating is placed outside the electrode group relative to the second coating when forming the electrode group; the first coating includes the first plane area 3 and the first winding area 2; the second coating includes the second plane area 5 and the second winding area 4. The coating length of the first coating is greater than the coating length of the negative electrode second coating.

[0036] The coating amount of the first winding area is greater than the coating amount of the first plane area, which can improve the N / P ratio of the negative electrode first coating layer facing the positive electrode sheet and effectively prevent lithium deposition.

[0037] The coating amount of the second winding area is less than the coating amount of the second plane area, thereby reducing the proportion of the negative electrode active material content in the battery.

[0038] For ease of implementation, the coating amount of the first planar area is usually equal to the coating amount of the second planar area.

[0039] The coating amount of the first plane area is 10-30 mg / cm 2 , specifically 10 mg / cm 2 , 20mg / cm 2 、30mg / cm 2 The coating amount in the first winding area is 0.7-2 mg / cm higher than that in the first plane area. 2 , specifically 0.7 mg / cm 2 , 1mg / cm 2 , 2mg / cm 2 .

[0040] Preferably, the coating amount of the second plane area is 10-30 mg / cm 2 , specifically 10 mg / cm 2 , 20mg / cm 2 、30mg / cm 2 The coating amount of the second winding area is 0.5-1.0 mg / cm lower than that of the second flat area.2 , specifically 0.5 mg / cm 2 , 0.7mg / cm 2 , 1mg / cm 2 .

[0041] The present invention also includes a method for preparing the negative electrode sheet, comprising the following steps: preparing negative electrode slurry; coating the negative electrode slurry on both sides of the negative electrode current collector to obtain a first coating and a second coating, and then drying, rolling and shearing to prepare the negative electrode sheet.

[0042] The negative electrode slurry comprises a negative electrode active material, a negative electrode conductive agent, a negative electrode dispersant, and a negative electrode binder;

[0043] The mass ratio of the negative electrode active material, the negative electrode conductive agent, the negative electrode dispersant, and the negative electrode binder is (90-98): (0.1-2): (0.1-4): (1-4), specifically 90:2:4:4, 98:0.1:0.9:1, or 97:1:1:1, etc.;

[0044] Preferably, the negative electrode active material is artificial graphite; the conductive agent is one or more of conductive carbon black and carbon nanotubes;

[0045] Preferably, the negative electrode dispersant is sodium carboxymethyl cellulose.

[0046] Preferably, the negative electrode binder is styrene-butadiene rubber latex.

[0047] Figure 4-5 A pole group is shown, comprising the negative pole sheet 10, the positive pole sheet 20 and a separator; the first coating of the negative pole sheet is placed outside the pole group relative to the second coating when the pole group is formed.

[0048] The positive electrode sheet is prepared in the following manner: positive electrode active material: positive electrode conductive agent: positive electrode binder are added to an organic solvent in a mass ratio of (90-98): (1-5): (1-5), vacuumed and mixed and stirred in a blender to prepare a positive electrode slurry, and then coated, rolled and sheared to prepare a positive electrode sheet. The mass ratio of positive electrode active material: positive electrode conductive agent: positive electrode binder can be 90:2:4:4, 98:0.1:0.9:1 or 95:1:2:2.

[0049] The coating amount of positive electrode active material is 15-50mg / cm 2 ; Specifically, it can be 15mg / cm 2 , 20mg / cm 2 、30mg / cm 2 、50mg / cm 2 .

[0050] Preferably, the positive electrode active material is a lithium cobalt oxide material, a nickel-cobalt-manganese ternary material, a lithium manganate material or a lithium iron phosphate material, the positive electrode conductive agent is one or more of conductive carbon black and carbon nanotubes; the positive electrode binder is one or more of a homopolymer or copolymer of polyvinylidene fluoride;

[0051] Preferably, the drying temperature is 70°C-130°C, specifically 70°C, 80°C, 120°C, or 130°C.

[0052] The present invention also includes a lithium ion battery, including the electrode group and the electrolyte; the lithium ion battery is prepared by the following method: the positive electrode sheet, the negative electrode sheet and the separator are prepared into an electrode group by winding, and the lithium ion battery is prepared by aluminum-plastic packaging, liquid injection, standing, pressurizing, and degassing;

[0053] Preferably, the manufactured lithium-ion battery is subjected to a cycle test, where the battery is charged at 1C until fully charged and then rested for 10 minutes, and then discharged at 1C. After the charge and discharge are repeated 500 times, the battery is fully charged and disassembled to observe whether there is obvious lithium deposition at the negative electrode.

[0054] Preferably, the thickness of the aluminum-plastic is 110-160um, specifically 110um, 130um, 160um; the temperature of battery formation is 70℃-95℃, specifically it can be adjusted to 70℃, 80℃, 90℃ according to needs; preferably, the temperature range of the injection process is 18-26℃, specifically it can be adjusted to 18℃, 20℃, 26℃ according to needs; it does not exceed 12h from the start to the end of injection; preferably, the environment for disassembling the battery requires a dew point temperature of less than -34.5 degrees Celsius.

[0055] The following is an exemplary description using preferred embodiments.

[0056] Example 1

[0057] A method for preparing a lithium ion battery, the specific steps are as follows:

[0058] (1) Preparation of positive electrode sheet: according to the mass percentage, lithium cobalt oxide: conductive carbon black: carbon nanotube: polyvinylidene fluoride copolymer = 95:1:2:2 is put into the slurry tank. After stirring, the prepared positive electrode slurry is dispersed at high speed and then enters the coating process. The coating amount of the positive electrode sheet is 39.5mg / cm 2 , after coating, drying at 110°C, rolling and shearing, the positive electrode sheet is made;

[0059] (2) Preparation of negative electrode sheet: According to the mass percentage, artificial graphite: conductive agent: sodium carboxymethyl cellulose: styrene butadiene rubber latex = 97:1:1:1, after stirring, prepare the negative electrode slurry. In the coating process, first use a double-layer nozzle to coat the first flat area 3 and the first winding area 2 ( Figure 1 ), after drying at 80°C, the negative electrode second plane area 5 and the second winding area 4 ( Figure 3 ), dried at 80°C, rolled and sheared to form a negative electrode sheet;

[0060] The coating amount of the negative electrode first winding area of ​​the negative electrode sheet is 17.6 mg / cm 2 The coating amount of the first plane area and the second plane area of ​​the negative electrode is 16.9 mg / cm 2 The coating amount of the negative electrode second winding area is 16.2 mg / cm 2 ;

[0061] (3) Lithium-ion battery production, winding the positive electrode sheet, negative electrode sheet, separator, tab and other battery materials into an electrode group ( Figure 4-5 As shown, a 113 μm thick aluminum plastic is selected, and the shell is punched into a suitable size, and the battery is manufactured through assembly, liquid injection, etc. The formation temperature is 80°C, and the battery is prepared after formation and degassing.

[0062] (4) The battery is charged and discharged at 1C: charged to 4.2V at 1C, then switched to constant voltage charging with a cut-off current of 0.02C, and then discharged at 1C to 3.0V after 10 minutes of sleep, and then rested for 10 minutes. After 500 cycles, the battery is disassembled and the disassembled battery is in a fully charged state. After disassembly, it can be observed that the negative electrode of the battery is in normal condition without lithium precipitation.

[0063] Example 2

[0064] A method for preparing a lithium ion battery, the specific steps are as follows:

[0065] (1) Preparation of positive electrode sheet: according to the mass percentage, lithium cobalt oxide: conductive carbon black: carbon nanotube: polyvinylidene fluoride copolymer = 95:1:2:2 is put into the slurry tank. After stirring, the prepared positive electrode slurry is dispersed at high speed and then enters the coating process. The coating amount of the positive electrode sheet is 39.5mg / cm 2 , after coating, drying at 110°C, rolling and shearing, the positive electrode sheet is made;

[0066] (2) Preparation of negative electrode sheet: According to the mass percentage, artificial graphite: conductive agent: sodium carboxymethyl cellulose: styrene-butadiene rubber latex = 97:1:1:1, after stirring, prepare the negative electrode slurry. In the coating process, first use a double-layer nozzle to coat the first plane area and the first winding area, dry at 80°C, then coat the second plane area and the second winding area of ​​the negative electrode, dry at 80°C, roll and shear to form the negative electrode sheet;

[0067] The coating amount of the negative electrode first winding area of ​​the negative electrode sheet is 18.5 mg / cm 2The coating amount of the first and second plane areas of the negative electrode is 17.5 mg / cm 2 The coating amount of the negative electrode second winding area is 16.5 mg / cm 2 ;

[0068] (3) Battery production: The positive electrode sheet, negative electrode sheet, separator, tab and other battery materials are wound into an electrode group. A 113 μm thick aluminum plastic is selected and punched into a shell of appropriate size. The battery is manufactured through assembly, liquid injection and other chemical processes. The chemical formation temperature is 80°C. After chemical formation and degassing, the battery is completed.

[0069] (4) The battery is charged and discharged at 1C: charged to 4.2V at 1C, then switched to constant voltage charging with a cut-off current of 0.02C, and then discharged at 1C to 3.0V after 10 minutes of sleep, and then rested for 10 minutes. After 500 cycles, the battery is disassembled and the disassembled battery is in a fully charged state. After disassembly, it can be observed that the negative electrode of the battery is in normal condition without lithium precipitation.

[0070] Example 3

[0071] A method for preparing a lithium ion battery, the specific steps are as follows:

[0072] (1) Preparation of positive electrode sheet: according to the mass percentage, lithium cobalt oxide: conductive carbon black: carbon nanotube: polyvinylidene fluoride copolymer = 95:1:2:2 is put into the slurry tank. After stirring, the prepared positive electrode slurry is dispersed at high speed and then enters the coating process. The coating amount of the positive electrode sheet is 39.5mg / cm 2 , after coating, drying at 110°C, rolling and shearing, the positive electrode sheet is made;

[0073] (2) Preparation of negative electrode sheet: According to the mass percentage, artificial graphite: conductive agent: sodium carboxymethyl cellulose: styrene-butadiene rubber latex = 97:1:1:1, after stirring, prepare the negative electrode slurry. In the coating process, first use a double-layer nozzle to coat the first plane area and the first winding area, dry at 80°C, then coat the second plane area and the second winding area of ​​the negative electrode, dry at 80°C, roll and shear to form the negative electrode sheet;

[0074] The coating amount of the negative electrode first winding area of ​​the negative electrode sheet is 18.0 mg / cm2, the coating amount of the negative electrode first and second plane areas is 17.5 mg / cm2, and the coating amount of the negative electrode second winding area is 17.0 mg / cm2;

[0075] (3) Battery production: The positive and negative electrodes, separators, tabs and other battery materials are wound into an electrode group. A 113 μm thick aluminum plastic is selected and punched into a shell of appropriate size. The battery is manufactured through assembly, liquid injection and other chemical processes. The formation temperature is 80°C. After formation and degassing, the battery is completed.

[0076] (4) The battery is charged and discharged at 1C: charged to 4.2V at 1C, then switched to constant voltage charging with a cut-off current of 0.02C, and then discharged at 1C to 3.0V after 10 minutes of sleep, and then rested for 10 minutes. After 500 cycles, the battery is disassembled and the disassembled battery is in a fully charged state. After disassembly, it can be observed that the negative electrode of the battery is in normal condition without lithium precipitation.

[0077] Comparative Example 1

[0078] Take the positive electrode sheet in step (1) of case 1, the first plane area, the second plane area, the first winding area, and the second winding area of ​​the negative electrode sheet with a uniform coating amount of 16.9 mg / cm 2 , after winding, packaging, formation, exhaust, etc., it was made into a battery. It was charged and discharged at 1C for 500 cycles, and then disassembled after being fully charged. After disassembly, there was slight lithium deposition at the outer corner of the negative electrode sheet.

[0079] The results of the above implementation cases and comparative cases are shown in Table 1 below, where the plane area is the value of the first plane area and the second plane area, which are the same; Difference 1 is the difference between the first winding area and the first plane area; Difference 2 is the difference between the first winding area and the first plane area; When the coating amount of the second winding area is lower than the coating amount of the second plane area by 0.5-1.0 mg / cm 2 When doing so, we can ensure that the energy density difference is not large, and we will not go into details.

[0080] Table 1

[0081]

[0082] In summary, the negative electrode sheet of the present application, by using the coating amount of the first winding area to be greater than the coating amount of the first plane area, can increase the N / P ratio of the first coating of the negative electrode facing the positive electrode sheet, and effectively prevent lithium precipitation. At the same time, since the coating amount of the second winding area of ​​the negative electrode is less than the coating amount of the second plane area of ​​the negative electrode, the proportion of the negative electrode active material content in the battery is reduced. As a result, the entire electrode group can effectively prevent lithium precipitation in the winding area of ​​the battery without affecting the energy density of the battery, thereby improving the safety performance of the battery.

[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A negative electrode sheet, characterized in that: It includes a current collector and a first coating and a second coating coated on both sides of the current collector; the first coating and the second coating respectively and independently include a plane area and a winding area arranged at intervals; the plane area and the winding area respectively correspond to the plane area and the winding area of ​​the electrode group formed by winding the negative electrode sheet; when forming the electrode group, the first coating is placed on the outside of the electrode group relative to the second coating; the first coating includes a first plane area and a first winding area; the second coating includes a second plane area and a second winding area.

2. The negative electrode sheet according to claim 1, characterized in that: The coating amount of the first winding area is greater than the coating amount of the first plane area.

3. The negative electrode sheet according to claim 1, characterized in that: The coating amount of the second winding area is smaller than that of the second plane area.

4. The negative electrode sheet according to claim 1, characterized in that: The coating amount of the first plane area is equal to the coating amount of the second plane area; preferably, the coating length of the first coating is greater than the coating length of the negative electrode second coating.

5. The negative electrode sheet according to claim 1, characterized in that: The coating amount of the first plane area is 10-30 mg / cm 2 , and the coating amount of the first winding area is higher than that of the first flat area by 0.7-2 mg / cm 2 . Preferably, the coating amount of the second plane area is 10-30 mg / cm 2 , and the coating amount of the second winding area is 0.5-1.0mg / cm lower than that of the second plane area 2 .

6. A method for preparing a negative electrode sheet according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: preparing negative electrode slurry; coating the negative electrode slurry on both sides of the negative electrode current collector to obtain a first coating layer and a second coating layer, and then drying, rolling and shearing to prepare a negative electrode sheet.

7. The method for preparing a negative electrode sheet according to claim 6, characterized in that: The negative electrode slurry comprises a negative electrode active material, a negative electrode conductive agent, a negative electrode dispersant, and a negative electrode binder; The mass ratio of the negative electrode active material, the negative electrode conductive agent, the negative electrode dispersant, and the negative electrode binder is (90-98): (0.1-2): (0.1-4): (1-4); Preferably, the negative electrode active material is artificial graphite; the conductive agent is one or more of conductive carbon black and carbon nanotubes; Preferably, the negative electrode dispersant is sodium carboxymethyl cellulose. Preferably, the negative electrode binder is styrene-butadiene rubber latex.

8. A pole group, characterized in that: It comprises a positive electrode sheet and the negative electrode sheet, a positive electrode sheet and a separator as claimed in any one of claims 1 to 7; the first coating of the negative electrode sheet is placed outside the electrode group relative to the second coating when forming the electrode group.

9. The pole group according to claim 8, characterized in that: The positive electrode sheet is prepared by the following method: adding positive electrode active material: positive electrode conductive agent: positive electrode binder in a mass ratio of (90-98): (1-5): (1-5) to an organic solvent, evacuating and mixing and stirring in a blender to prepare a positive electrode slurry, and then coating, rolling and shearing to prepare a positive electrode sheet; Preferably, the coating amount of the positive electrode active material is 15-50 mg / cm 2 . Preferably, the positive electrode active material is a lithium cobalt oxide material, a nickel-cobalt-manganese ternary material, a lithium manganate material or a lithium iron phosphate material, the positive electrode conductive agent is one or more of conductive carbon black and carbon nanotubes; the positive electrode binder is one or more of a homopolymer or copolymer of polyvinylidene fluoride; Preferably, the drying temperature is 70°C-130°C.

10. A lithium ion battery, characterized in that: The invention comprises the electrode group and the electrolyte as described in any one of claims 8 to 9; the lithium-ion battery is prepared by the following method: the positive electrode sheet, the negative electrode sheet and the separator are prepared into an electrode group by winding, and the lithium-ion battery is prepared by aluminum-plastic packaging, liquid injection, standing, pressurizing and degassing; Preferably, the manufactured lithium-ion battery is subjected to a cycle test, where the battery is charged at 1C until fully charged and then rested for 10 minutes, and then discharged at 1C. After the charge and discharge are repeated 500 times, the battery is fully charged and disassembled to observe whether there is obvious lithium deposition at the negative electrode. Preferably, the thickness of the aluminum-plastic is 110-160um, and the temperature of the battery formation is 70°C-95°C; preferably, the temperature range of the injection process is 18-26°C, and the time from the start of injection to the end of injection does not exceed 12 hours; preferably, the environment for disassembling the battery requires a dew point temperature less than -34.5 degrees Celsius.