Preparation method and application of hierarchical pore monolithic catalyst with high specific surface area

Through interface-induced redox radical polymerization method and postpolymerization modification, a monolithic catalyst with high specific surface area and multi-stage pore structure was prepared, which solved the problems of complex process and uneven loading of active components in the prior art, and achieved the The effect of efficient catalysis and simplification of the process is achieved.

CN118925805APending Publication Date: 2024-11-12CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972996.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyHIPE-based monolithic catalyst has complex processes, uneven loading of active components, low mass transfer efficiency, and insufficient catalytic activity.

Method used

The porous monolithic column was prepared by interfacially induced redox radical polymerization method, and the monolithic catalyst with high specific surface area and multi-stage porous structure was obtained through postpolymerization modification and in-situ loading of metal nanoparticles.

Benefits of technology

It realizes efficient catalytic reduction reaction, improves catalytic activity and conversion efficiency, simplifies the preparation process, and has practical feasibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004953762490000011
    Figure HDA0004953762490000011
  • Figure HDA0004953762490000012
    Figure HDA0004953762490000012
  • Figure HDA0004953762490000013
    Figure HDA0004953762490000013
Patent Text Reader

Abstract

The invention belongs to the technical field of catalytic material carriers, and particularly relates to a preparation method and application of a hierarchical pore monolithic catalyst with a high specific surface area. According to the invention, divinyl benzene is taken as a monomer, a pore-foaming agent is introduced into a continuous phase, and a novel method for regulating and controlling a foam structure through polymerization kinetics is provided, namely, a high-molecular nano-aggregate is formed at an oil-water interface through oxidation-reduction free radical polymerization initiated by the interface, and finally, through post-polymerization modification and metal nanoparticle in-situ loading, the foam structure is obtained. The monolithic catalyst with a high specific surface area and a hierarchical pore structure is obtained. The monolithic catalyst with high specific surface area and hierarchical pore structure prepared by the invention can realize continuous catalytic reduction pointer reaction, quickly mix the components, accurately control the reaction temperature and time and improve the conversion efficiency, and the preparation method is simple and has practical feasibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic material carriers, and in particular relates to a preparation method and application of a high specific surface area, multi-level porous monolithic catalyst. Background Art

[0002] Porous polymer materials have good application prospects in the fields of catalysis, gas adsorption, chemical separation, drug loading, etc. due to their high specific surface area, low-density skeleton and high chemical and physical stability. At present, the common preparation methods of porous polymer materials include electrospinning, direct template method, block copolymer self-assembly method, gas foaming method, freeze drying method and emulsion template method.

[0003] The emulsion template method provides an effective way to customize the pore structure and porosity, and the open pore size, pore structure and porosity of the carrier can be precisely controlled by the dispersed phase morphology. At the same time, the emulsion template is gel-like and can be cast into any shape and size, and the template is easy to remove after polymerization. The internal phase volume fraction of the emulsion used in the emulsion template method is generally greater than 74.05%, so it is defined as a high internal phase emulsion (HIPE). By polymerizing the external phase (continuous phase) of HIPE, a polymer skeleton is obtained, and the internal phase is removed as a pore structure, and finally a porous polymer monolithic material (polyHIPE) is obtained.

[0004] PolyHIPE materials have a high degree of connectivity in their internal pore structure and high porosity. They can be post-polymerized and loaded with catalytically active components to obtain monolithic catalytic materials, which have good application prospects in the field of catalysis. Some Chinese patents have focused on the application of polyHIPE materials as monolithic catalyst carriers. For example, Chinese patent (ZL201510812566.9) focuses on the possible application of polystyrene-based porous materials as adsorption materials and catalyst carrier materials; Chinese patent (ZL201910965655.5) uses poly(p-chloromethylstyrene) porous materials to induce in-situ mineralization of silicon and aluminum sources to obtain macroporous-mesoporous silicon-aluminum composite carriers, which can be used to prepare C5 petroleum resin hydrogenation catalysts; Chinese patent (ZL 202010854662.0) used silica-stabilized Pickering high internal phase emulsion as a template to prepare polystyrene-based materials, and then obtained metallized porous polymer foams through sulfonation and metal electroless deposition, which have application value in catalytic degradation; Chinese patent (ZL201910156441.3) and Chinese patent (ZL202210379018.1) introduced covalent organic frameworks (COFs) and metal organic frameworks (MOFs) into polyHIPE, respectively, to prepare integral catalysts.

[0005] However, the process of the above-mentioned polyHIPE-based monolithic catalyst is relatively complicated, the active component loading is uneven, and the obtained monolithic catalyst has low mass transfer efficiency and insufficient catalytic activity. Summary of the invention

[0006] The purpose of the present invention is to provide a preparation method and application of a high specific surface area, multi-level porous monolithic catalyst, directly using divinylbenzene as a monomer, introducing different porogens into the continuous phase, and proposing a new method for regulating the pore structure by polymerization kinetics, that is, preparing a porous monolithic column by interface-initiated redox free radical polymerization, and finally obtaining a monolithic catalyst with a high specific surface area and a multi-level porous structure by post-polymerization modification and in-situ loading of metal nanoparticles, and confirming that the monolithic catalyst can efficiently catalyze and reduce continuous pointer reactions. The method is simple to prepare and has practical feasibility.

[0007] The method for preparing the high specific surface area, multi-level porous monolithic catalyst adopted by the invention comprises the preparation of the porous monolithic column and the loading of the active components.

[0008] Furthermore, the porous monolithic column is prepared by an emulsion template method, comprising the following steps:

[0009] Divinylbenzene, porogen, oil-soluble oxidant and emulsifier are mixed by oscillation to form a continuous phase, and a water-soluble reducing agent, electrolyte and water are mixed by oscillation to form a dispersed phase. The dispersed phase is added to the continuous phase in small amounts and multiple times under the action of a high-speed shearing machine to obtain a high internal phase emulsion, which is transferred to an oven for polymerization, and then purified and dried to obtain a monolithic porous material;

[0010] Among them, the mass proportions of each raw material are: continuous phase and dispersed phase, the continuous phase contains 5 to 16 parts of divinylbenzene, 1 to 12 parts of porogen, 0.1 to 0.5 parts of oil-soluble oxidant and 1 to 5 parts of emulsifier, the dispersed phase contains 0.5 to 1 part of electrolyte, 0.2 to 1.5 parts of water-soluble reducing agent, and 70 to 89 parts of water.

[0011] Furthermore, the porogen includes any one of aromatic hydrocarbons, alkanes and cycloalkanes, such as toluene, xylene, hexane, heptane, octane, nonane, decane, cyclohexane, cycloheptane, cyclooctane and the like.

[0012] Further, the emulsifier includes Span 80, Span 60, Aldo 33, Emcol EL-50, Emcol PP-50, Emcol PM-50, Emcol PL-50, Emcol DO-50, Emcol DP-50, Atlas G-2859, Atlas G-2146, Atlas G-917, Atlas G-2139 and Atlas G-1702.

[0013] Furthermore, the electrolyte is an inorganic salt, including sodium chloride, potassium chloride, calcium chloride, sodium sulfate, calcium sulfate and the like.

[0014] Further, the oil-soluble oxidant includes any one of benzoyl peroxide (BPO), tert-butyl peroxy-2-ethylhexanoate (TBPO), isopropylbenzene hydroperoxide (CHP), azobisisobutyronitrile (AIBN), azobisisoheptanenitrile (V65), azobisisovaleronitrile (V59), dimethyl azobisisobutyrate (V601), etc.

[0015] Furthermore, the water-soluble reducing agent includes any one of tetramethylethylenediamine (TEMED), ascorbic acid (AA), ferrous sulfate, stannous chloride, sodium sulfite and the like.

[0016] Furthermore, the mass ratio of the oil-soluble oxidizing agent to the water-soluble reducing agent is 1:1 to 1:5.

[0017] Furthermore, the shear rate of the high-speed shearing machine is 5000-15000 rpm, and the shear time is 5-20 min.

[0018] Furthermore, the polymerization temperature is 50 to 90° C., and the polymerization time is 6 to 48 hours.

[0019] Furthermore, the loading of the active components includes introducing active anchor points through post-polymerization modification and in-situ loading of active components.

[0020] Furthermore, the post-polymerization modification includes any one of nitration-ammoniation, sulfonation and chemical grafting. The chemical grafting includes chemical grafting of compounds containing carboxylate, sulfonate, phosphate and other groups. The residual double bonds and / or active hydrogen of the benzene ring of polydivinylbenzene are used to introduce active anchor points such as amino, sulfonate and carboxylate.

[0021] Furthermore, the in-situ loaded active component is a noble metal nanoparticle, including any one of gold, silver, palladium, platinum, etc. The active anchor points on the monolithic porous material skeleton form ion pairs and / or ligands with the noble metal ions, and the in-situ noble metal ions obtain a monolithic catalyst loaded with noble metal nanoparticles.

[0022] Beneficial technical effects achieved by the present invention:

[0023] The present invention uses interfacial redox free radical polymerization to place the oxidant and the reductant in the oil phase and the water phase respectively. When they come into contact at the oil-water interface, a redox reaction occurs to generate free radicals, which initiate the polymerization of monomers. It can accurately and quickly form polymer nano-aggregates at the oil-water interface, and finally obtain a high specific surface area, porous-grade monolithic porous material with a specific surface area of ​​more than 400m 2 / g, which is beneficial to post-polymerization modification, in-situ loading of noble metal nanoparticles and material transfer during the reaction process.

[0024] The monolithic catalyst prepared by the present invention has a multi-level pore structure, wherein the through macropores of the emulsion template method can promote the transmission and mixing of the reaction substrate, and the micro / mesopores induced by the polymerization reaction can provide sites for catalytic conversion. Finally, the multi-level pore structure synergistically catalyzes the reduction of the pointer reaction continuously, and combines the material conveying equipment and the temperature control component to accurately control the material residence time and the reaction temperature, thereby improving the conversion efficiency of the chemical reaction. For example, the monolithic catalyst prepared in the exemplary embodiment of the present invention can achieve 90% catalytic conversion of 4-nitrophenol within 18 minutes. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope image of the porous monolithic column described in Example 1 (with a macropore distribution statistical diagram embedded);

[0026] Figure 2 The nitrogen adsorption-desorption curve (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 1;

[0027] Figure 3 This is a scanning electron microscope image of the porous monolithic column described in Example 2 (with a macropore distribution statistical diagram embedded);

[0028] Figure 4 The nitrogen adsorption-desorption curve (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 2;

[0029] Figure 5 This is a scanning electron microscope image of the porous monolithic column described in Example 3;

[0030] Figure 6 The nitrogen adsorption-desorption curve diagram (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 3;

[0031] Figure 7 This is a scanning electron microscope image of the porous monolithic column described in Example 4;

[0032] Figure 8 The nitrogen adsorption-desorption curve (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 4;

[0033] Fig. 9 This is a scanning electron microscope image of the porous monolithic column described in Example 5;

[0034] Fig.10 The nitrogen adsorption-desorption curve diagram (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 5;

[0035] Fig.11This is a scanning electron microscope image of the porous monolithic column described in Example 6;

[0036] Fig.12 The nitrogen adsorption-desorption curve diagram (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 6;

[0037] Fig.13 This is a scanning electron microscope image of the porous monolithic column described in Example 7;

[0038] Fig.14 The nitrogen adsorption-desorption curve (left) and micro / mesopore distribution diagram (right) of the porous monolithic column described in Example 7;

[0039] Fig.15 This is a scanning electron microscope image of the porous monolithic column described in Comparative Example 1;

[0040] Fig.16 This is a scanning electron microscope image of the porous monolithic column described in Comparative Example 2;

[0041] Fig.17 This is a scanning electron microscope image of the porous monolithic column described in Comparative Example 3. DETAILED DESCRIPTION

[0042] The present invention is further described in detail with the following examples, but the embodiments of the present invention are not limited thereto.

[0043] Embodiment 1:

[0044] The specific implementation steps are as follows:

[0045] (1) 12 parts of divinylbenzene, 6 parts of toluene, 0.2 parts of BPO and 2 parts of Span 80 were mixed by oscillation to form a continuous phase, and 0.6 parts of ascorbic acid, 1.0 parts of sodium chloride and 78.7 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000 rpm and the shear time was 15 min to obtain a high internal phase emulsion, which was transferred to a 60°C oven for polymerization for 12 hours, purified and dried to obtain a porous monolithic column (PH-1).

[0046] (2) 1 g of PH-1 was added to 4 mL of acetic anhydride and 40 mL of DCE (dichloroethane) to swell, and stirred at room temperature overnight; the swollen PH-1 was cooled in an ice-water bath, 5 mL of concentrated nitric acid (concentration of about 68%) at 4°C was added, the ice bath was removed, the temperature was gradually raised to room temperature, and then raised to 75°C for reaction for 5 hours. After the reaction was completed, it was cooled to room temperature, the porous monolithic column was clamped out, and it was repeatedly washed with acetic acid and ethanol, and then washed with a large amount of deionized water until neutral, and dried; the porous monolithic column was added to a mixed solution of 20 mL of acetic anhydride, 1 g of SnCI2 and 1.5 mL of HCI (35.6-38 wt%), and stirred at 25°C for reaction for 72 hours, and then the porous monolithic column was clamped out, and it was repeatedly washed with a mixed solution of acetic acid and hydrochloric acid in a ratio of 4:1, and then washed with a sodium hydroxide solution with a mass fraction of 5%, and finally washed with deionized water until neutral, and vacuum dried to obtain an amino-modified porous monolithic column (PH-NH2-1).

[0047] (3) Finally, the silver mirror reaction between amino groups and silver ions was used to achieve in-situ loading of silver nanoparticles to obtain a monolithic catalyst (PH-Ag-1). The specific experimental method was to take 1 part of PH-NH2-1 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of silver nitrate aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of diethanolamine (30.0 mg mL -1 ), react at 70°C for 2h, collect the product, wash and vacuum dry.

[0048] The specific surface area of ​​the monolithic catalyst in Example 1 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table Figure 1 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Figure 2 .

[0049] Embodiment 2:

[0050] The specific implementation steps are as follows:

[0051] (1) 12 parts of divinylbenzene, 6 parts of octane, 0.2 parts of BPO and 2 parts of Aldo 33 were mixed by oscillation to form a continuous phase, and 0.6 parts of ascorbic acid, 1.0 parts of potassium chloride and 78.7 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000 rpm and the shear time was 15 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 6 hours, purified and dried to obtain a porous monolithic column (PH-2).

[0052] (2) Under nitrogen protection, 12.4 mL of acetic anhydride, 6.8 mL of concentrated sulfuric acid and 24 mL of 1,2-dichloroethane were added to a 100 mL three-necked flask that was fully dried and pre-cooled with ice water, respectively, and the mixture was stirred and reacted at 0° C. for 2 hours to obtain a 1,2-dichloroethane solution of acetylsulfuric acid;

[0053] 1 g of PH-2 and 50 mL of 1,2-dichloroethane were stirred and heated to 50°C. After the solid was completely dissolved, 10 mL of acetylsulfuric acid solution was slowly added dropwise to the reaction bottle. After the addition was complete, the reaction was continued for 5 hours. The mixture was cooled to room temperature and then poured into 200 mL of n-hexane. The porous monolithic column was clipped out and dried under vacuum to obtain a sulfonate-modified porous monolithic column (PH-SO3H-2).

[0054] (3) The in-situ loading of palladium nanoparticles was achieved by utilizing the ion pairing and in-situ reduction of sulfonate and palladium ions to obtain a monolithic catalyst (PH-Pd-2). The specific experimental method was to take 1 part of PH-SO3H-2 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of palladium chloride aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 30°C for 2h, collect the product, wash and vacuum dry.

[0055] The specific surface area of ​​the monolithic catalyst in Example 2 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 1. Figure 3 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Figure 4 .

[0056] Embodiment 3:

[0057] The specific implementation steps are as follows:

[0058] (1) 12 parts of divinylbenzene, 6 parts of cyclohexane, 0.2 parts of BPO and 2 parts of Emcol PM-50 were mixed by oscillation to form a continuous phase, and 0.6 parts of ascorbic acid, 1.0 parts of calcium chloride and 78.4 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000 rpm and the shear time was 15 min to obtain a high internal phase emulsion, which was transferred to a 90°C oven for polymerization for 24 hours, purified and dried to obtain a porous monolithic column (PH-3).

[0059] (2) In a 250 mL round-bottom flask, a condenser was installed, 20 mL of a reaction solvent water-ethanol mixed solution was added, 1 g PH-3, 0.5 g cysteine, and 0.032 g azobisisobutyronitrile were added, and the mixture was slowly stirred to be evenly dispersed. Then, the temperature was raised to 65°C in a nitrogen atmosphere, and the mixture was reacted for 12 hours. After cooling to room temperature, the porous monolithic column was clamped out, and the reaction solution was added to wash it three times. After that, it was washed three times with tetrahydrofuran, acetone, and anhydrous ether, and then vacuum dried in a vacuum drying oven at 50°C for 24 hours to obtain a carboxylate-modified porous monolithic column (PH-COOH-3).

[0060] (3) Using the ion pairing and in-situ reduction of carboxylate and platinum ions, in-situ loading of platinum nanoparticles was achieved to obtain a monolithic catalyst (PH-Pt-3). The specific experimental method was to take 1 part of PH-COOH-3 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of platinum tetrachloride aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 30°C for 2h, collect the product, wash and vacuum dry to obtain a monolithic catalyst.

[0061] The specific surface area of ​​the monolithic catalyst in Example 3 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 2. Figure 5 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Figure 6 .

[0062] Embodiment 4:

[0063] The specific implementation steps are as follows:

[0064] (1) 12 parts of divinylbenzene, 6 parts of octane, 0.2 parts of BPO and 2 parts of Aldo 33 were mixed by oscillation to form a continuous phase, and 0.2 parts of ascorbic acid, 1.0 parts of potassium chloride and 78.7 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000 rpm and the shear time was 15 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 6 hours, purified and dried to obtain a porous monolithic column (PH-4).

[0065] (2) As in Example 1, an amino-modified porous monolithic column (PH-NH2-4) was obtained.

[0066] (3) Finally, the pairing effect of amino groups and gold ions was used to achieve in-situ loading of gold nanoparticles to obtain a monolithic catalyst (PH-Au-4). The specific experimental method was to take 1 part of PH-NH2-4 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of chloroauric acid solution (10.0 mg mL -1), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 70°C for 2h, collect the product, wash and vacuum dry.

[0067] The specific surface area of ​​the monolithic catalyst in Example 4 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 1. Figure 7 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Figure 8 .

[0068] Embodiment 5:

[0069] The specific implementation steps are as follows:

[0070] (1) 12 parts of divinylbenzene, 6 parts of octane, 0.2 parts of BPO and 2 parts of Aldo 33 were mixed by oscillation to form a continuous phase, and 1.0 part of ascorbic acid, 1.0 part of potassium chloride and 78.1 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000 rpm and the shear time was 15 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 6 hours, purified and dried to obtain a porous monolithic column (PH-5).

[0071] (2) As in Example 1, an amino-modified porous monolithic column (PH-NH2-5) was obtained.

[0072] (3) Finally, the silver mirror reaction between amino groups and silver ions was used to achieve in-situ loading of silver nanoparticles to obtain a monolithic catalyst (PH-Ag-5). The specific experimental method was to take 1 part of PH-NH2-5 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of silver nitrate aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of diethanolamine (30.0 mg mL -1 ), react at 70°C for 2h, collect the product, wash and vacuum dry.

[0073] The specific surface area of ​​the monolithic catalyst in Example 5 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 2. Fig. 9 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Fig.10 .

[0074] Embodiment 6:

[0075] The specific implementation steps are as follows:

[0076] (1) 12 parts of divinylbenzene, 6 parts of xylene, 0.3 parts of AIBN and 2 parts of Atlas G-2146 were mixed by oscillation to form a continuous phase, and 0.9 parts of ferrous sulfate, 1.0 parts of sodium sulfate and 78.1 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 15000 rpm and the shear time was 20 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 48 hours, purified and dried to obtain a porous monolithic column (PH-6).

[0077] (2) As in Example 1, an amino-modified porous monolithic column (PH-NH2-6) was obtained.

[0078] (3) Finally, the pairing effect of amino groups and gold ions was used to achieve in-situ loading of gold nanoparticles to obtain a monolithic catalyst (PH-Au-6). The specific experimental method was to take 1 part of PH-NH2-6 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of chloroauric acid solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 70°C for 2h, collect the product, wash and vacuum dry.

[0079] The specific surface area of ​​the monolithic catalyst in Example 6 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 1. Fig.11 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Fig.12 .

[0080] Embodiment 7:

[0081] The specific implementation steps are as follows:

[0082] (1) 12 parts of divinylbenzene, 6 parts of xylene, 0.3 parts of V601 and 2 parts of Emcol PP-50 were mixed by oscillation to form a continuous phase, and 0.9 parts of TEMED, 1.0 parts of calcium sulfate and 78.1 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 5000 rpm and the shear time was 5 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 12 hours, purified and dried to obtain a porous monolithic column (PH-7).

[0083] (2) As in Example 2, a sulfonate-modified porous monolithic column (PH-SO3H-7) was prepared;

[0084] (3) Using the ion pairing and in-situ reduction of sulfonate and palladium ions, the in-situ loading of palladium nanoparticles was achieved to obtain a monolithic catalyst (PH-Pd-7). The specific experimental method was to take 1 part of PH-SO3H-7 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of palladium chloride aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 30°C for 2h, collect the product, wash and vacuum dry.

[0085] The specific surface area of ​​the monolithic catalyst in Example 7 is shown in Table 1, and its cross-sectional morphology and macropore distribution are shown in Table 1. Fig.13 , nitrogen adsorption-desorption curves and micro / mesopore distribution are shown in Fig.14 .

[0086] Comparative Example 1:

[0087] The specific implementation steps are as follows:

[0088] 10 parts of divinylbenzene, 8 parts of heptane and 2 parts of Emcol DO-50 were mixed by oscillation to form a continuous phase, and 0.3 parts of VA-061, 0.7 parts of sodium chloride and 79 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 10000rpm and the shear time was 15min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 12h, purified and dried to obtain a porous monolithic column (DPH-1).

[0089] The specific surface area of ​​the porous monolithic column in Comparative Example 1 is shown in Table 1, and its cross-sectional morphology is shown in Table Fig.15 .

[0090] Comparative Example 2

[0091] The specific implementation steps are as follows:

[0092] (1) 10 parts of divinylbenzene, 8 parts of heptane and 2 parts of Atlas G-2146 were mixed by oscillation to form a continuous phase, and 1.0 part of sodium chloride and 89 parts of water were mixed by oscillation to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase was added to the continuous phase in small amounts and multiple times, wherein the shear rate was 15000 rpm and the shear time was 20 min to obtain a high internal phase emulsion, which was transferred to a 75°C oven for polymerization for 12 hours, purified and dried to obtain a porous monolithic column (DPH-2).

[0093] (2) As in Example 3, a carboxylate-modified porous monolithic column (DPH-COOH-2) was prepared.

[0094] (3) Using the ion pairing and in-situ reduction of carboxylate and platinum ions, the in-situ loading of platinum nanoparticles was achieved to obtain a monolithic catalyst (DPH-Pt-2). The specific experimental method was to take 1 part of DPH-COOH-2 and fully swell it in 80 parts of deionized water (12 h), add 10 parts of platinum tetrachloride aqueous solution (10.0 mg mL -1 ), and after sufficient stirring, add 10 parts of sodium borohydride (30.0 mg mL -1 ), react at 30°C for 2h, collect the product, wash and vacuum dry.

[0095] The specific surface area of ​​the monolithic porous material in Comparative Example 2 is shown in Table 1, and its cross-sectional morphology is shown in Table Fig.16 .

[0096] Comparative Example 3:

[0097] The specific implementation steps are as follows:

[0098] (1) 49 parts of divinylbenzene, 40 parts of trichlorobenzene, 10 parts of Atlas G-2139 and 1 part of AIBN were mixed by oscillation. The mixed solution was transferred to a 75°C oven for polymerization for 12 hours, purified and dried to obtain a monolithic material.

[0099] (2) As in Example 3, a carboxylate-modified porous monolithic column was obtained.

[0100] (3) As in Example 3, a monolithic catalyst was obtained.

[0101] The specific surface area of ​​the monolithic porous material in Comparative Example 3 is shown in Table 1, and its cross-sectional morphology is shown in Table 1. Fig.17 .

[0102] Catalytic performance test

[0103] 4-nitrophenol was used to simulate industrial wastewater containing oxygen. Taking Example 2 as an example, in static catalysis, 0.5 mL of sodium borohydride aqueous solution (0.2 M) was added to a mixture of 4.5 mL of 4-nitrophenol aqueous solution (0.1 mM) and 10 mg of the monolithic catalyst to carry out a catalytic reduction reaction. Samples were taken at 1, 3, 5, 7, 10, 12, 15, and 45 min for UV-visible spectrum analysis, and the conversion efficiency was recorded as the time when 90% of the 4-nitrophenol was converted. The catalytic efficiencies of all the examples and comparative examples are shown in Table 1.

[0104] Placing the monolithic catalyst in a continuous flow catalytic system can carry out long-term and continuous catalytic reduction reactions.

[0105] Table 1 shows the micropore-mesopore parameters of Examples 1 to 7 and Comparative Examples 1 to 3.

[0106] Table 1

[0107] sample <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Total pore volume (cm 3 / g)]]> Average pore size (nm) Conversion time (min) Example 1 313 0.69 17.2 25 Example 2 421 1.12 18.3 18 Example 3 349 0.83 18.7 23 Example 4 361 0.87 17.5 20 Example 5 344 0.82 18.5 21 Example 6 375 0.94 18.4 22 Example 7 396 0.74 21.6 19 Comparative Example 1 386 0.68 10.26 No catalytic activity Comparative Example 2 146 0.31 6.63 54 Comparative Example 3 104 0.28 5.21 76

[0108] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a monolithic catalyst for continuous catalytic reduction, It is characterized in that The steps include: (1) divinylbenzene, a porogen, an oil-soluble oxidant and an emulsifier are vibrated and mixed to form a continuous phase, and a water-soluble reducing agent, an electrolyte and water are vibrated and mixed to form a dispersed phase. Under the action of a high-speed shearing machine, the dispersed phase is added to the continuous phase to obtain a high internal phase emulsion, which is transferred to an oven for polymerization reaction, and then purified and dried to obtain a porous monolithic column; (2) Post-polymerization modification of the porous monolithic column; (3) Loading active components to obtain an integral catalyst.

2. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1, It is characterized in that The mass fractions of the raw materials described in step (1) are: 5 to 16 parts of divinylbenzene, 1 to 12 parts of porogen, 0.1 to 0.5 parts of oil-soluble oxidant, 1 to 5 parts of emulsifier, 0.5 to 1 part of electrolyte, 0.2 to 1.5 parts of water-soluble reducing agent, and 70 to 89 parts of water.

3. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1 or 2, It is characterized in that The oil-soluble oxidant includes any one of benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, cumene hydroperoxide, azobisisobutyronitrile, azobisisoheptanenitrile, azobisisovaleronitrile, and dimethyl azobisisobutyrate.

4. A method for preparing a monolithic catalyst for continuous catalytic reduction according to claim 1 or 2, It is characterized in that The water-soluble reducing agent includes any one of tetramethylethylenediamine, ascorbic acid, ferrous sulfate, stannous chloride and sodium sulfite.

5. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1 or 2, It is characterized in that The mass ratio of the oil-soluble oxidant to the water-soluble reducing agent is 1:1 to 1:

5.

6. A method for preparing a monolithic catalyst for continuous catalytic reduction according to claim 1 or 2, It is characterized in that The porogen includes toluene, xylene, hexane, heptane, octane, nonane, decane, cyclohexane, cycloheptane, and cyclooctane; The emulsifiers include Span 80, Span 60, Aldo 33, Emcol EL-50, Emcol PP-50, Emcol PM-50, Emcol PL-50, Emcol DO-50, Emcol DP-50, Atlas G-2859, Atlas G-2146, Atlas G-917, Atlas G-2139, and Atlas G-1702; The electrolyte is an inorganic salt, including sodium chloride, potassium chloride, calcium chloride, sodium sulfate, and calcium sulfate.

7. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1, It is characterized in that The shear rate of the high-speed shearing machine is 5000-15000 rpm, and the shearing time is 5-20 min; The polymerization temperature is 50-90° C., and the polymerization time is 6-48 hours.

8. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1, It is characterized in that The post-polymerization modification includes any one of nitration-ammoniation, sulfonation and chemical grafting; the chemical grafting includes chemical grafting of compounds containing carboxylate, sulfonate and phosphate.

9. The method for preparing the monolithic catalyst for continuous catalytic reduction according to claim 1, It is characterized in that The in-situ loaded active component is a noble metal nanoparticle, including any one of gold, silver, palladium and platinum.

10. Use of a monolithic catalyst prepared according to the method according to any one of claims 1 to 9 in catalytic reduction of 4-nitrophenol.