Method for preparing environment-friendly antibacterial fiberboard from tobacco stems

By simulating the lignification process of plants, environmentally friendly antibacterial fiberboard is prepared by using the reaction of tobacco stems with mustard alcohol glucoside and laccase, which solves the problem of formaldehyde pollution in traditional fiberboards, and realizes the efficient resource utilization of tobacco stem waste and the fiberboard. Antibacterial properties.

CN118927368APending Publication Date: 2024-11-12HUBEI CHINA TOBACCO INDUSTRY CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411300530.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The phenolic resin and urea formaldehyde resin used in the traditional fiberboard preparation method will release formaldehyde, resulting in environmental pollution and health hazards, and it is difficult to achieve efficient resource utilization of tobacco stem waste.

Method used

Using tobacco stems as raw material, through water immersion, wire rub, refinement, dilution and mixing reaction with mustard alcohol glucoside and laccase, the plant lignification process is simulated, and the crosslinking of covalent bonds such as anisole bond and ester bond are formed. , prepare environmentally friendly antibacterial fiberboard to avoid the use of chemical additives.

Benefits of technology

The preparation of environmentally friendly fiberboard without formaldehyde pollution is achieved, which gives fiberboard antibacterial properties, and improves the utilization rate of tobacco stem waste, providing an environmentally friendly and pollution-free resource utilization method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the field of resource utilization of tobacco raw materials, and particularly relates to a method for preparing an environment-friendly antibacterial fiberboard from tobacco stems, which comprises the following steps: a) dipping the tobacco stems in water, rolling threads, and grinding to obtain crude tobacco stem pulp; b) diluting the crude tobacco stem pulp with a sodium acetate-acetic acid buffer solution with the pH value of 3-5, and then mixing the diluted crude tobacco stem pulp with glucosinolate and laccase for reaction to obtain treated tobacco stem pulp; c) forming the treated tobacco stem pulp on a net to obtain a wet plate blank; and d) carrying out hot pressing on the wet plate blank to obtain the environment-friendly antibacterial fiberboard. According to the method, the tobacco stems serve as raw materials for preparing the fiberboard, and resource utilization of tobacco stem waste is achieved; according to the method, phenolic aldehyde, urea formaldehyde and other resin materials do not need to be added in the fiberboard preparation process, and the formaldehyde pollution problem of a traditional fiberboard preparation method is fundamentally solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resource utilization of tobacco raw materials, and in particular relates to a method for preparing environmentally friendly antibacterial fiberboards by utilizing tobacco stems. Background Art

[0002] Fiberboard is a polymer composite material made of plant fibers bonded by phenolic resin and urea-formaldehyde resin. Compared with synthetic polymer products, fiberboard not only has good strength, durability and dimensional stability, but also has good environmental compatibility as a natural polymer material. However, since phenolic resin and urea-formaldehyde resin will release free formaldehyde during use, it will cause serious harm to people's life and health, especially when used for interior decoration, it often becomes an invisible "killer". Formaldehyde can combine with amino groups in proteins, denature proteins, disrupt cell metabolism, have a great destructive effect on human cells, and can cause cancer. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a method for preparing environmentally friendly antibacterial fiberboard using tobacco stems. This method uses tobacco stems as raw materials for preparing fiberboard, thereby realizing the resource utilization of tobacco stem waste; and this method does not require the addition of resin materials such as phenolic formaldehyde and urea formaldehyde during the preparation of fiberboard, thereby fundamentally eliminating the formaldehyde pollution problem of traditional fiberboard preparation methods.

[0004] The present invention provides a method for preparing an environmentally friendly antibacterial fiberboard using tobacco stems, comprising the following steps:

[0005] a) soaking the tobacco stems in water, rolling them into threads, and grinding them to obtain a rough pulp of tobacco stems;

[0006] b) diluting the tobacco stem crude pulp with a sodium acetate-acetic acid buffer solution having a pH of 3 to 5, and then mixing and reacting with sinapyl glucoside and laccase to obtain a treated tobacco stem pulp;

[0007] c) placing the treated tobacco stem slurry on a screen to form a wet slab;

[0008] d) The wet slab is hot pressed to obtain an environmentally friendly antibacterial fiberboard.

[0009] Preferably, in step a), the material-liquid ratio of the impregnation is 1 g:(5-10) mL; the impregnation temperature is 60-80° C.; and the impregnation time is 5-10 h.

[0010] Preferably, in step a), the thread rolling slurry concentration is 30-40wt%; and the thread rolling time is 30-60min.

[0011] Preferably, in step a), the pulp concentration of the pulping is 30-40 wt%; and the beating degree of the tobacco stem pulp obtained after the pulping is 15-25° SR.

[0012] Preferably, in step b), the concentration of the diluted slurry is 3-6 wt %.

[0013] Preferably, in step b), the amount of sinapyl glucoside used is 0.5-1 g / L slurry.

[0014] Preferably, in step b), the laccase is added to the reaction system in the form of a laccase solution; the enzyme activity of the laccase solution is 20 to 50 U / g; and the dosage of the laccase solution is 2 to 5 mL / L slurry.

[0015] Preferably, in step b), the reaction temperature is 40-60° C.; and the reaction time is 2-3 h.

[0016] Preferably, in step c), the moisture content of the wet slab is 40-50 wt%.

[0017] Preferably, in step d), the temperature of the hot pressing is 200-250°C.

[0018] Preferably, in step d), the hot pressing includes a high-pressure water squeezing section, a drying section and a plasticizing section in sequence; wherein the pressure of the high-pressure water squeezing section is 4 to 6 MPa, and the time is 6 to 10 min; the pressure of the drying section is 2 to 4 MPa, and the time is 6 to 10 min; the pressure of the plasticizing section is 3 to 6 MPa, and the time is 10 to 15 min.

[0019] Compared with the prior art, the present invention provides a method for preparing environmentally friendly antibacterial fiberboard using tobacco stems, comprising the following steps: a) soaking the tobacco stems in water, rolling and grinding to obtain tobacco stem coarse pulp; b) diluting the tobacco stem coarse pulp with a sodium acetate-acetic acid buffer solution with a pH of 3 to 5, and then mixing and reacting with sinapinic acid glucoside and laccase to obtain treated tobacco stem slurry; c) forming the treated tobacco stem slurry on a net to obtain a wet slab; d) hot pressing the wet slab to obtain an environmentally friendly antibacterial fiberboard. The present invention simulates the lignification process of plants, and uses a lignin oxidase system to catalyze the free radical polymerization reaction between the residual lignin, sinapyl glucoside and carbohydrates in the fiber, so that the separated fibers regenerate crosslinking in the form of lignin-polysaccharide complexes such as anisole bonds and ester bonds, and covalent bonds such as Beta-aryl ether bonds between lignin, so that the tobacco stem fibers form a strong chemical bond crosslinking, and a layer of lignin-like substances grows again on the fiber surface, so that not only lignin can be deposited between the fibers, but also part of the pectin polysaccharide can be deposited, thereby achieving the repair of the fiber intercellular layer in the true sense, and finally achieving the enhancement of the degradable "green" material based on plant fiber by the enzyme catalytic polymerization system, and fundamentally eliminating the formaldehyde pollution problem caused by the traditional method. The method provided by the present invention uses tobacco stems with a high pectin content as raw materials, and no chemical additives are added in the process of preparing fiberboards, and sinapyl glucoside with antibacterial effect is added, the preparation process is environmentally friendly and pollution-free, the fiberboard is given antibacterial properties, and the utilization rate of tobacco stem waste can be improved. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The present invention provides a method for preparing an environmentally friendly antibacterial fiberboard using tobacco stems, comprising the following steps:

[0022] a) soaking the tobacco stems in water, rolling them into threads, and grinding them to obtain a rough pulp of tobacco stems;

[0023] b) diluting the tobacco stem crude pulp with a sodium acetate-acetic acid buffer solution having a pH of 3 to 5, and then mixing and reacting with sinapyl glucoside and laccase to obtain a treated tobacco stem pulp;

[0024] c) placing the treated tobacco stem slurry on a screen to form a wet slab;

[0025] d) The wet slab is hot pressed to obtain an environmentally friendly antibacterial fiberboard.

[0026] In the method provided by the present invention, in step a), the pectin content of the tobacco stems is preferably 10-15wt%, specifically 10wt%, 10.5wt%, 11wt%, 11.5wt%, 12wt%, 12.5wt%, 13wt%, 13.5wt%, 14wt%, 14.5wt% or 15wt%.

[0027] In the method provided by the present invention, in step a), the material-liquid ratio (mass volume ratio of tobacco stems to water) of the impregnation is preferably 1g:(5-10)mL, specifically 1g:5mL, 1g:5.5mL, 1g:6mL, 1g:6.5mL, 1g:7mL, 1g:7.5mL, 1g:8mL, 1g:8.5mL, 1g:9mL, 1g:9.5mL or 1g:10mL; the impregnation temperature is preferably 60-80°C, specifically 60°C, 65°C, 70°C, 75°C or 80°C; the impregnation time is preferably 5-10h, specifically 5h, 6h, 7h, 8h, 9h or 10h.

[0028] In the method provided by the present invention, in step a), the thread rolling is preferably carried out using a twin screw; the slurry concentration of the thread rolling is preferably 30-40wt%, specifically 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%; the thread rolling time is preferably 30-60min, specifically 30min, 35min, 40min, 45min, 50min, 55min or 60min.

[0029] In the method provided by the present invention, in step a), the slurry concentration of the refining is preferably 30-40wt%, specifically 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%; the beating degree of the tobacco stem pulp obtained after the refining is preferably 15-25°SR, specifically 15°SR, 16°SR, 17°SR, 18°SR, 19°SR, 20°SR, 21°SR, 22°SR, 23°SR, 24°SR or 25°SR.

[0030] In the method provided by the present invention, in step b), the pH of the sodium acetate-acetic acid buffer solution can be specifically 3, 3.5, 4, 4.5 or 5.

[0031] In the method provided by the present invention, in step b), the concentration of the diluted slurry is preferably 3-6wt%, specifically 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt% or 6wt%.

[0032] In the method provided by the present invention, in step b), the dosage of sinapyl glucoside is preferably 0.5-1 g / L slurry, specifically 0.5 g / L slurry, 0.6 g / L slurry, 0.7 g / L slurry, 0.8 g / L slurry, 0.9 g / L slurry or 1 g / L slurry.

[0033] In the method provided by the present invention, in step b), the laccase is preferably added to the reaction system in the form of a laccase liquid; the enzyme activity of the laccase liquid is preferably 20-50 U / g, specifically 20 U / g, 25 U / g, 30 U / g, 35 U / g, 40 U / g, 45 U / g or 50 U / g; the dosage of the laccase liquid is preferably 2-5 mL / L slurry, specifically 2 mL / L slurry, 2.5 mL / L slurry, 3 mL / L slurry, 3.5 mL / L slurry, 4 mL / L slurry, 4.5 mL / L slurry or 5 mL / L slurry.

[0034] In the method provided by the present invention, in step b), the reaction temperature is preferably 40-60°C, specifically 40°C, 45°C, 50°C, 55°C or 60°C; the reaction time is preferably 2-3h, specifically 2h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h or 3h.

[0035] In the method provided by the present invention, in step c), before the treated tobacco stem slurry is put on the screen for forming, its concentration is preferably adjusted to 0.75-1.5wt%, specifically 0.75wt%, 1wt%, 1.25wt% or 1.5wt%.

[0036] In the method provided by the present invention, in step c), during the process of forming on the net, it is preferred to use rollers to pressurize and dehydrate and control the thickness of the slab.

[0037] In the method provided by the present invention, in step c), the moisture content of the wet slab is preferably 40-50wt%, specifically 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% or 50wt%.

[0038] In the method provided by the present invention, in step d), the temperature of the hot pressing is preferably 200-250°C, specifically 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C or 250°C.

[0039] In the method provided by the present invention, in step d), the hot pressing preferably includes a high-pressure water squeezing section, a drying section and a plasticizing section in sequence; wherein the pressure of the high-pressure water squeezing section is preferably 4-6 MPa, specifically 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa or 6 MPa, and the time of the high-pressure water squeezing section is preferably 6-10 min, specifically 6 min, 7 min, 8 min, 9 min or 10 min; the pressure of the drying section is preferably 2-4 MPa, specifically 2 MPa, 2.5 MPa, 3 MPa, 3.5 MPa or 4 MPa, and the time of the drying section is preferably 6-10 min, specifically 6 min, 7 min, 8 min, 9 min or 10 min. The plasticizing period can be 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min or 10 min; the pressure of the plasticizing section is preferably 3-6 MPa, specifically 3 MPa, 3.5 MPa, 4 MPa, 4.5 MPa, 5 MPa, 5.5 MPa or 6 MPa; the time of the plasticizing section is preferably 10-15 min, specifically 10 min, 10.5 min, 11 min, 11.5 min, 12 min, 12.5 min, 13 min, 13.5 min, 14 min, 14.5 min or 15 min.

[0040] The method provided by the present invention simulates the lignification process of plants, and uses a lignin oxidase system to catalyze the free radical polymerization reaction between the residual lignin, sinapyl glucoside and carbohydrates in the fiber, so that the separated fibers regenerate crosslinking in the form of lignin-polysaccharide complexes such as anisole bonds and ester bonds, and covalent bonds such as Beta-aryl ether bonds between lignins, so that the tobacco stem fibers form a strong chemical bond crosslinking, and a layer of lignin-like substances grows again on the fiber surface, so that not only lignin can be deposited between the fibers, but also part of the pectin polysaccharide can be deposited, thereby achieving the repair of the fiber intercellular layer in the true sense, and finally achieving the enhancement of the degradable "green" material based on plant fibers by the enzyme catalytic polymerization system, and fundamentally eliminating the formaldehyde pollution problem caused by the traditional method. The method provided by the present invention uses tobacco stems with a high pectin content as raw materials, and no chemical additives are added in the process of preparing fiberboards, and sinapyl glucoside with antibacterial effect is added, the preparation process is environmentally friendly and pollution-free, the fiberboard is given antibacterial properties, and the utilization rate of tobacco stem waste can be improved.

[0041] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0042] Example 1

[0043] (1) Preparation of tobacco stem slurry by twin-screw extruder: Tobacco stem (pectin content 12 wt%) was soaked in hot water (temperature 60°C, time 5 h, solid-liquid ratio 1 g:5 mL), twisted by twin-screw extruder (pulp concentration 30 wt%, time 30 min), and high-concentration grinding by disc grinding (pulp concentration 30 wt%, beating degree 15° SR);

[0044] (2) Tobacco stem fiber treatment: Sodium acetate-acetic acid buffer with a pH of 3 was added to dilute the tobacco stem slurry to a concentration of 3 wt%. The fiber suspension was stirred and mixed with an electric stirrer at a temperature of 40°C. A certain amount of sinapyl glucoside (0.5 g / L) and laccase solution (enzyme activity 20 U / g, 2 mL / L) were added and kept warm for 2 h.

[0045] (3) Wet slab preparation: A vacuum single-cylinder type was used to prepare the wet slab. The slurry concentration was 0.75 wt%. The slurry was adsorbed on the cylindrical screen by vacuum action, and the slab thickness was controlled by roller pressure dehydration. The moisture content of the wet slab was 40%;

[0046] (4) Preparation of fiberboard by hot pressing: hot pressing temperature is 200°C, high pressure water squeezing section pressure is 4 MPa, time is 6 min, drying section pressure is 2 MPa, time is 6 min, plasticizing section pressure is 3 MPa, time is 10 min.

[0047] Example 2

[0048] (1) Preparation of tobacco stem slurry by twin-screw extruder: Tobacco stem (pectin content 12 wt%) was soaked in hot water (temperature 70°C, time 8 h, solid-liquid ratio 1 g:8 mL), twisted by twin-screw extruder (pulp concentration 35 wt%, time 45 min), and high-concentration grinding by disc grinding (pulp concentration 35 wt%, beating degree 20° SR);

[0049] (2) Tobacco stem fiber treatment: Sodium acetate-acetic acid buffer with a pH of 4 was added to dilute the tobacco stem slurry to a concentration of 5 wt %. The fiber suspension was stirred and mixed with an electric stirrer at a temperature of 50° C. A certain amount of sinapyl glucoside (0.75 g / L) and laccase solution (enzyme activity 35 U / g, 3.5 mL / L) were added, and the reaction was kept warm for 2.5 h.

[0050] (3) Wet slab preparation: A vacuum single-cylinder type was used to prepare the wet slab. The slurry concentration was 1.0 wt %. The slurry was adsorbed on the cylindrical screen by vacuum action, and the slab thickness was controlled by roller pressure dehydration. The moisture content of the wet slab was 45%;

[0051] (4) Preparation of fiberboard by hot pressing: hot pressing temperature is 230°C, high pressure water squeezing section pressure is 5 MPa, time is 8 min, drying section pressure is 3 MPa, time is 8 min, plasticizing section pressure is 4.5 MPa, time is 12 min.

[0052] Example 3

[0053] (1) Preparation of tobacco stem slurry by twin-screw extruder: Tobacco stem (pectin content 12 wt%) was soaked in hot water (temperature 80°C, time 10 h, solid-liquid ratio 1 g:10 mL), twisted by twin-screw extruder (pulp concentration 40 wt%, time 60 min), and high-concentration grinding by disc grinding (pulp concentration 40 wt%, beating degree 25° SR);

[0054] (2) Tobacco stem fiber treatment: Sodium acetate-acetic acid buffer with a pH of 5 was added to dilute the tobacco stem slurry to a concentration of 6 wt %. The fiber suspension was stirred and mixed with an electric stirrer at a temperature of 60° C. A certain amount of sinapyl glucoside (1 g / L) and laccase solution (enzyme activity 50 U / g, 5 mL / L) were added, and the reaction was kept warm for 3 h.

[0055] (3) Wet slab preparation: A vacuum single-cylinder type was used to prepare the wet slab. The slurry concentration was 1.5 wt%. The slurry was adsorbed on the cylindrical screen by vacuum action, and the slab thickness was controlled by roller pressure dehydration. The moisture content of the wet slab was 50%;

[0056] (4) Preparation of fiberboard by hot pressing: hot pressing temperature is 250°C, high pressure water squeezing section pressure is 6 MPa, time is 10 min, drying section pressure is 4 MPa, time is 10 min, plasticizing section pressure is 6 MPa, time is 15 min.

[0057] Comparative Example 1

[0058] (1) Preparation of tobacco stem slurry by twin-screw extruder: Tobacco stem (pectin content 12 wt%) was soaked in hot water (temperature 60°C, time 5 h, solid-liquid ratio 1 g:5 mL), twisted by twin-screw extruder (pulp concentration 30 wt%, time 30 min), and high-concentration refining by disc grinding (pulp concentration 30%, beating degree 15° SR);

[0059] (2) Tobacco stem fiber treatment: sodium acetate-acetic acid buffer with a pH of 3 was added to dilute the tobacco stem slurry to a concentration of 3 wt %, and the fiber suspension was stirred and mixed with an electric stirrer at a temperature of 40° C.;

[0060] (3) Wet slab preparation: A vacuum single-cylinder type was used to prepare the wet slab. The slurry concentration was 0.75 wt%. The slurry was adsorbed on the cylindrical screen by vacuum action, and the slab thickness was controlled by roller pressure dehydration. The moisture content of the wet slab was 40%;

[0061] (4) Preparation of fiberboard by hot pressing: hot pressing temperature is 200°C, high pressure water squeezing section pressure is 4 MPa, time is 2 min, pressure holding is 4 min, drying section pressure is 2 MPa, time is 6 min, plasticizing section pressure is 3 MPa, time is 10 min.

[0062] Performance Evaluation

[0063] (1) Static bending strength analysis (three-point bending)

[0064] The static bending strength of three-point bending is measured by applying a load to the middle of the specimen supported at two points. It is to determine the ratio of the bending moment and the bending section modulus of the specimen when the maximum load is applied. Cut a specimen of size 15mm×200mm and place the specimen in an environment with a temperature of (20±2)℃ and a relative humidity of (65±5)% until the mass is constant. The mass is considered constant if the difference between the two weighing results 24 hours apart does not exceed 0.1% of the mass of the specimen. Adjust the span of the two supports to at least 20 times the basic thickness of the specimen, and measure the center distance of the supports to an accuracy of 0.5mm. The specimen is placed flat on the support, with the long axis of the specimen perpendicular to the support roller and the center point of the specimen below the loading roller.

[0065] Load at a constant rate throughout the test. Adjust the loading speed so that the maximum load is reached within (60 ± 30) s. Record the maximum load to the nearest 1% of the measured value.

[0066] The static bending strength of the sample is calculated according to the following formula, accurate to 0.1MPa:

[0067]

[0068] Where:

[0069] ρ b ——static bending strength of the specimen, in megapascals (MPa);

[0070] F max ——The maximum load when the specimen fails, in Newton (N);

[0071] l1——the distance between two supports, in millimeters (mm);

[0072] b——specimen width, in millimeters (mm);

[0073] t——specimen thickness, in millimeters (mm).

[0074] (2) Internal bonding strength measurement

[0075] Internal bond strength is the measurement of the tensile strength of the sample surface when it is subjected to uniformly distributed tensile force until it is destroyed. Internal bond strength is the ratio of the maximum destructive tensile force perpendicular to the sample surface to the sample area.

[0076] Apply epoxy resin glue or melted hot melt glue or similar adhesive evenly on the surface of the chuck to bond the specimen to the chuck. Remove the glue squeezed out of the glue layer. Place the assembly in the clamping device and load until the specimen fails. The entire test should be loaded evenly, and the specimen should fail within (60±30)s from the start of loading. Record the maximum load value with an accuracy of 1%.

[0077] The internal bonding strength is calculated according to the following formula:

[0078]

[0079] Where:

[0080] σ ⊥ ——Internal bond strength of the specimen, in megapascals (MPa);

[0081] F max ——The maximum load when the specimen fails, in Newton (N);

[0082] l——specimen length, in millimeters (mm);

[0083] b——specimen width, in millimeters (mm).

[0084] (3) Antibacterial experiment

[0085] ① Prepare LB (beef extract peptone) solution

[0086] Tryptone 10g / L; NaCl 10g / L; Yeast 5g / L; pH = 7.0-7.4

[0087] ②Sample preparation

[0088] The felt prepared in the examples and the common felt were made into circular samples with a diameter of 6 mm.

[0089] ③Sterilization operation

[0090] Wrap the culture dish, spreader, deionized water (put in a conical flask), LB solution, and LB solution with 2% agar (20 g / L) (100 mL in each conical flask) in newspaper, place in an autoclave, and sterilize at 121°C for 45 minutes.

[0091] ④ Activation of E. coli

[0092] Take 100 μL of the frozen Escherichia coli and put it in 5 mL of LB culture medium. Place the culture solution on a shaker at 37°C and 200 r / min. Take it out after 12 hours. Then take 100 μL of the above culture solution and put it in 5 mL of LB culture medium. Place the culture solution on a shaker at 37°C and 200 r / min. Take it out after 2-3 hours.

[0093] ⑤Measure OD value

[0094] Take 1mL of the cultured bacterial solution, centrifuge at 8000r / min for 5min, pour off the supernatant and add 3mL of water, stir evenly and measure the absorbance of the bacterial solution in a UV spectrophotometer at 600nm, then dilute the bacterial solution (sterile water) to 5~5*106cfu / mL (1OD=1*109cfu / mL)

[0095] ⑥ Experimental steps

[0096] Place the above disinfected instruments and samples on a sterile workbench and irradiate with ultraviolet light for 30 minutes. Then pour the LB solution into the culture dish, about 30 mL each, and then let it stand for 15 minutes until the agar solidifies. Take 200 μL of the diluted bacterial solution in the culture dish, rotate the culture dish to evenly distribute the bacterial solution on the surface, let it stand for about 15 minutes, and stick the sample on the surface of the culture medium, with 3 pieces of fiberboard samples in the example attached to each dish. Cover the culture dish with a lid, seal it with a sealing film, and put it in an incubator at 37.5°C. After 7 hours, observe and measure the diameter of the antibacterial zone around the filter paper and keep a record.

[0097] (4) Test results:

[0098]

[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing environmentally friendly antibacterial fiberboard using tobacco stems, It is characterized in that The following steps are involved: a) soaking the tobacco stems in water, rolling them into threads, and grinding them to obtain a rough pulp of tobacco stems; b) diluting the tobacco stem crude pulp with a sodium acetate-acetic acid buffer solution having a pH of 3 to 5, and then mixing and reacting with sinapyl glucoside and laccase to obtain a treated tobacco stem pulp; c) placing the treated tobacco stem slurry on a screen to form a wet slab; d) The wet slab is hot pressed to obtain an environmentally friendly antibacterial fiberboard.

2. The method according to claim 1, It is characterized in that In step a), the material-liquid ratio of the impregnation is 1 g: (5-10) mL; the impregnation temperature is 60-80° C.; and the impregnation time is 5-10 h.

3. The method according to claim 1, It is characterized in that In step a), the thread rolling slurry concentration is 30-40wt%; the thread rolling time is 30-60min.

4. The method according to claim 1, It is characterized in that In step a), the pulp concentration of the pulping is 30-40wt%; the beating degree of the tobacco stem pulp obtained after the pulping is 15-25°SR.

5. The method according to claim 1, It is characterized in that In step b), the concentration of the diluted slurry is 3-6 wt %.

6. The method according to claim 1, It is characterized in that In step b), the dosage of sinapyl glucoside is 0.5-1 g / L slurry.

7. The method according to claim 1, It is characterized in that In step b), the laccase is added to the reaction system in the form of a laccase solution; the enzyme activity of the laccase solution is 20-50 U / g; and the dosage of the laccase solution is 2-5 mL / L slurry.

8. The method according to claim 1, It is characterized in that In step b), the reaction temperature is 40-60° C. and the reaction time is 2-3 h.

9. The method according to claim 1, It is characterized in that In step c), the moisture content of the wet slab is 40-50wt%.

10. The method according to claim 1, It is characterized in that In step d), the temperature of the hot pressing is 200-250°C; The hot pressing includes a high-pressure water squeezing section, a drying section and a plasticizing section in sequence; wherein the pressure of the high-pressure water squeezing section is 4-6 MPa and the time is 6-10 min; the pressure of the drying section is 2-4 MPa and the time is 6-10 min; the pressure of the plasticizing section is 3-6 MPa and the time is 10-15 min.

Citation Information

Patent Citations

  • A biological treatment method to improve paper strength

    CN102296474A

  • Tobacco stalk fiber substance as well as preparation method and application thereof

    CN102475353A

  • Fabricating method of formaldehyde-free wheat straw medium density fiberboard

    CN102758384A

  • Method for enhancing paper strength based on enzymatic catalytic lignin dehydrogenized polymer

    CN106522013A

  • Antimicrobial and moisture-absorbing bath towel fabric

    CN108095617A