Perfluorohexanone microcapsule fire extinguishing medium and preparation process thereof

By modifying the combination of guar gum and porous silica, perfluorohexanone microcapsule fire extinguishing media is prepared, which solves the problem of insufficient heat resistance and stability in the prior art, and achieves efficient fire extinguishing performance and long-term stability sex.

CN118949336AActive Publication Date: 2024-11-15CHINA FIRE SAFETY TECH IND (SHENZHEN) CO LTD

Patent Information

Application Number
CN202411026243.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing perfluorohexanone microcapsule fire extinguishing media have poor heat resistance and long-term stability, making it difficult to effectively preserve and apply.

Method used

Modified guar gum as the shell material, and modified guar gum with porous silica as the core material by diphenylphosphinyl chloride, combined with acrylic resin, aluminum hydroxide and emulsifier, to prepare perfluorohexanone microcapsules Fire extinguishing medium improves the sealing effect and flame retardant performance of the shell.

Benefits of technology

The fire extinguishing performance, heat resistance and long-term stability of perfluorohexanone microcapsules are significantly improved, and volatilization is reduced, and excellent storage stability and efficient fire extinguishing performance are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968619210000021
    Figure BDA0004968619210000021
  • Figure BDA0004968619210000081
    Figure BDA0004968619210000081
  • Figure BDA0004968619210000091
    Figure BDA0004968619210000091
Patent Text Reader

Abstract

The invention discloses a perfluorohexanone microcapsule fire extinguishing medium and a preparation process thereof, and relates to the technical field of fire fighting. The perfluorohexanone microcapsule fire extinguishing medium is composed of a core material and a shell material, the core material comprises perfluorohexanone, silicon dioxide and azodiisobutyronitrile, and the shell material comprises modified guar gum, acrylic resin, aluminum hydroxide, potassium nitrate and an emulsifier; the modified guar gum is prepared by the following method: sequentially adding tetrahydrofuran, guar gum and triethylamine into a reactor, uniformly stirring and mixing, then dropwise adding a tetrahydrofuran solution of diphenyl phosphinyl chloride, heating to 75-85 DEG C after dropwise adding, reacting for 10-14 hours, and performing post-treatment to obtain the diphenyl phosphinyl chloride modified guar gum. The guar gum is modified through the diphenyl phosphinyl chloride, and then the modified guar gum is used as the shell material of the perfluorohexanone microcapsule, so that the fire extinguishing performance, the heat resistance and the long-acting stability of the perfluorohexanone microcapsule are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fire fighting, and in particular to a perfluorohexanone microcapsule fire extinguishing medium and a preparation process thereof. Background Art

[0002] Perfluorohexanone is a liquid under normal conditions with a boiling point of 49°C. It can quickly vaporize and volatilize at room temperature, making it difficult to store and use. Preparing perfluorohexanone into microcapsules and embedding them in polymer materials to form solid plastics is a good curing and application solution.

[0003] The Chinese invention patent with publication number CN 116271675 A discloses a perfluorohexanone microcapsule fire extinguishing medium and a preparation method thereof. Although the perfluorohexanone microcapsule fire extinguishing medium disclosed in the patent can extinguish a fire in more than 8 seconds, its heat resistance and long-term stability are relatively poor. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a perfluorohexanone microcapsule fire extinguishing medium and a preparation process thereof.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A perfluorohexanone microcapsule fire extinguishing medium, composed of a core material and a shell material, wherein the core material comprises perfluorohexanone, silicon dioxide, and azobisisobutyronitrile, and the shell material comprises modified guar gum, acrylic resin, aluminum hydroxide, potassium nitrate, and an emulsifier;

[0007] The modified guar gum is prepared by the following method:

[0008] Tetrahydrofuran, guar gum and triethylamine are added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride is added dropwise. After the addition is completed, the temperature is raised to 75-85°C for reaction for 10-14 hours, and post-processed to obtain guar gum modified with diphenylphosphinyl chloride. The reaction equation is shown as follows:

[0009]

[0010] Wherein, Guar Gum-OH represents guar gum, and OH represents the hydroxyl group on guar gum.

[0011] The mass ratio of the guar gum, triethylamine and diphenylphosphine chloride is 100:(10-15):(15-20).

[0012] The silicon dioxide is porous silicon dioxide with an average particle size of 400-800nm ​​and a specific surface area of ​​150-200m 2 / g.

[0013] The mass ratio of perfluorohexanone, silicon dioxide and azobisisobutyronitrile is 10:(2-3):(0.04-0.06).

[0014] The mass ratio of the modified guar gum, acrylic resin, aluminum hydroxide, potassium nitrate and emulsifier is 100:(6-10):(12-18):(1-2):(8-10).

[0015] A preparation process of perfluorohexanone microcapsule fire extinguishing medium comprises the following steps:

[0016] S1: adding perfluorohexanone, silicon dioxide and azobisisobutyronitrile into a reactor, stirring and mixing them thoroughly to obtain a perfluorohexanone fire extinguishing mixed liquid;

[0017] S2: adding deionized water, modified guar gum and potassium nitrate into a reactor, stirring and mixing, and obtaining an aqueous solution of modified guar gum;

[0018] S3: slowly adding the perfluorohexanone fire extinguishing mixed liquid, acrylic resin and emulsifier into the aqueous solution of modified guar gum, and stirring to obtain an emulsion;

[0019] S4: Add aluminum hydroxide to the emulsion, stir and mix, let stand for 2-6 hours, filter, wash with water, and freeze-dry to obtain perfluorohexanone microcapsule fire extinguishing medium.

[0020] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:

[0021] (1) The present invention modifies guar gum by using diphenylphosphine chloride, so that diphenylphosphine oxide groups are grafted onto the guar gum. The diphenylphosphine oxide groups are flame retardant groups. The modified guar gum is used as the shell material of perfluorohexanone microcapsules. On the one hand, the sealing effect of the shell material is improved, and the shell material itself has the performance of a flame retardant, thereby improving the fire extinguishing performance, heat resistance and long-term stability of the perfluorohexanone microcapsules.

[0022] (2) By using porous silica with an average particle size of 400-800nm ​​and a high specific surface area as the carrier of the perfluorohexanone fire extinguishing medium core material, its porous pore structure can carry perfluorohexanone and serve as its storage space, thereby reducing the contact area of ​​perfluorohexanone with the outside world. During the storage process, the volatilization of perfluorohexanone can be reduced. Therefore, the perfluorohexanone microcapsules prepared in this application have excellent heat resistance and long-term stability. DETAILED DESCRIPTION

[0023] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.

[0024] Example 1 Preparation of modified guar gum:

[0025] 200 g of tetrahydrofuran, 100 g of guar gum and 10 g of triethylamine were added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride was added dropwise (15 g of diphenylphosphinyl chloride was dissolved in 60 g of tetrahydrofuran and all added dropwise for 30 min). After the addition was completed, the temperature was raised to 75° C. and reacted for 14 h; filtered to remove insoluble salts, and evaporated at 60° C. to obtain guar gum modified with diphenylphosphinyl chloride.

[0026] Example 2 Preparation of modified guar gum:

[0027] 200 g of tetrahydrofuran, 100 g of guar gum and 12 g of triethylamine were added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride was added dropwise (18 g of diphenylphosphinyl chloride was dissolved in 70 g of tetrahydrofuran and all added dropwise for 30 min). After the addition was completed, the temperature was raised to 80° C. and reacted for 12 h; filtered to remove insoluble salts, and evaporated at 60° C. to obtain guar gum modified with diphenylphosphinyl chloride.

[0028] Example 3 Preparation of modified guar gum:

[0029] 200 g of tetrahydrofuran, 100 g of guar gum and 15 g of triethylamine were added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride was added dropwise (20 g of diphenylphosphinyl chloride was dissolved in 80 g of tetrahydrofuran and all added dropwise for 30 min). After the addition was completed, the temperature was raised to 85° C. and reacted for 10 h; filtered to remove insoluble salts, and evaporated at 60° C. to obtain guar gum modified with diphenylphosphinyl chloride.

[0030] Example 4 Preparation of perfluorohexanone microcapsule fire extinguishing medium:

[0031] S1: 300 g of perfluorohexanone, 60 g of porous silica (average particle size 780 nm, specific surface area 158 m 2 / g), 1.2g of azobisisobutyronitrile was added into the reactor, and stirred thoroughly to obtain a perfluorohexanone fire extinguishing mixed liquid;

[0032] S2: 250 g of deionized water, 100 g of modified guar gum (prepared in Example 1), and 1 g of potassium nitrate were added into a reactor, and stirred to mix well to obtain an aqueous solution of modified guar gum;

[0033] S3: slowly add 250 g of the perfluorohexanone fire extinguishing mixed liquid, 6 g of acrylic resin, and 8 g of emulsifier (SR-10) to the aqueous solution of modified guar gum in step S2, and stir at high speed to obtain an emulsion;

[0034] S4: Add 12 g of aluminum hydroxide to the emulsion of step S3, stir and mix, let stand for 2 h, filter with suction, wash the filter cake with 100 g of deionized water, and freeze-dry for 12 h to obtain perfluorohexanone microcapsule fire extinguishing medium.

[0035] Example 5 Preparation of perfluorohexanone microcapsule fire extinguishing medium:

[0036] S1: 300 g of perfluorohexanone, 75 g of porous silica (average particle size 640 nm, specific surface area 182 m 2 / g), 1.5g of azobisisobutyronitrile was added into the reactor, and stirred thoroughly to obtain a perfluorohexanone fire extinguishing mixed liquid;

[0037] S2: 250 g of deionized water, 100 g of modified guar gum (prepared in Example 2), and 1.5 g of potassium nitrate were added into a reactor, and stirred to obtain an aqueous solution of modified guar gum;

[0038] S3: slowly add 270 g of the perfluorohexanone fire extinguishing mixed liquid, 8 g of acrylic resin, and 9 g of emulsifier (SR-20) to the aqueous solution of modified guar gum in step S2, and stir at high speed to obtain an emulsion;

[0039] S4: Add 15 g of aluminum hydroxide to the emulsion of step S3, stir and mix, let stand for 5 hours, filter with suction, wash the filter cake with 90 g of deionized water, and freeze-dry for 12 hours to obtain perfluorohexanone microcapsule fire extinguishing medium.

[0040] Example 6 Preparation of perfluorohexanone microcapsule fire extinguishing medium:

[0041] S1: 300 g of perfluorohexanone, 90 g of porous silica (average particle size 410 nm, specific surface area 197 m 2 / g), 1.8g of azobisisobutyronitrile was added into the reactor, and stirred and mixed thoroughly to obtain a perfluorohexanone fire extinguishing mixed liquid;

[0042] S2: 250 g of deionized water, 100 g of modified guar gum (prepared in Example 3), and 2 g of potassium nitrate were added into a reactor, and stirred to mix well to obtain an aqueous solution of modified guar gum;

[0043] S3: slowly add 280g of perfluorohexanone fire extinguishing mixed liquid, 10g of acrylic resin, and 10g of emulsifier (SR-20) to the aqueous solution of modified guar gum in step S2, and stir at high speed to obtain an emulsion;

[0044] S4: Add 18 g of aluminum hydroxide to the emulsion of step S3, stir and mix, let stand for 6 hours, filter with suction, wash the filter cake with 80 g of deionized water, and freeze-dry for 12 hours to obtain perfluorohexanone microcapsule fire extinguishing medium.

[0045] Comparative Example 1

[0046] The preparation process of perfluorohexanone microcapsule fire extinguishing medium is basically the same as that of Example 5, except that the 100 g modified guar gum in step S2 is replaced by 85 g guar gum and 16 g diphenylphosphine chloride.

[0047] Comparative Example 2

[0048] The preparation process of perfluorohexanone microcapsule fire extinguishing medium is basically the same as that of Example 5, except that the 100 g modified guar gum in step S2 is replaced by 100 g guar gum.

[0049] Comparative Example 3

[0050] The preparation process of perfluorohexanone microcapsule fire extinguishing medium is basically the same as that of Example 5, except that the modified guar gum in step S2 is replaced by an equal weight of modified chitosan. The preparation method of modified chitosan is basically the same as that of Example 2, except that 100g of guar gum is replaced by 100g of chitosan.

[0051] Comparative Example 4

[0052] The preparation process of perfluorohexanone microcapsule fire extinguishing medium is basically the same as that of Example 5, except that the porous silica in step S1 is replaced by an equal weight of silica having an average particle size of 190 nm and a specific surface area of ​​219 m 2 / g of porous silica.

[0053] Comparative Example 5

[0054] The preparation process of perfluorohexanone microcapsule fire extinguishing medium is basically the same as that of Example 5, except that the porous silica in step S1 is replaced by an equal weight of silica with an average particle size of 980 nm and a specific surface area of ​​68 m 2 / g of porous silica.

[0055] Comparative Example 6

[0056] A perfluorohexanone microcapsule fire extinguishing medium prepared by the method of Example 2 of the Chinese invention patent publication number CN 116271675 A.

[0057] In the process of preparing perfluorohexanone microcapsule fire extinguishing medium in Examples 4-6 and Comparative Examples 1-5 of the present application, steps S1-S4 are all prepared at room temperature, where room temperature refers to 25° C., and the speed of high-speed stirring in step S3 is 1500 rpm and the stirring time is 30 min.

[0058] Preparation Example 1 of porous silica: silica (average particle size 640 nm, specific surface area 182 m 2 / g) preparation:

[0059] (1) adding fumed silica (average particle size 1000 nm) to a sand mill for grinding, controlling the sand mill speed to 8000 rpm, grinding time 50 min, and then drying the ground fumed silica in an oven at 80° C. for 7 h into powder;

[0060] (2) Weigh 50 g of formaldehyde solution (35 wt%) and 44 g of urea and stir evenly;

[0061] (3) Weigh 100 g of ground fumed silica powder and add it to the mixed solution of step (2), and stir evenly;

[0062] (4) adding 1500 g of deionized water to step (3) to dilute the solid content of the system, then adjusting the pH of the system to 1.0 with hydrochloric acid (2 M), and standing at room temperature for 24 h to obtain urea-formaldehyde resin-fumed silica composite nanospheres;

[0063] (5) filtering the urea-formaldehyde resin-fumed silica composite nanospheres, and then washing them four times with anhydrous ethanol (50 g each time) and deionized water (50 g each time), and drying them at 120° C. for 8 h to obtain urea-formaldehyde resin-fumed silica composite powders;

[0064] (6) The urea-formaldehyde resin-fumed silica composite powder was calcined at 600° C. for 6 h in a muffle furnace to obtain porous silica.

[0065] Preparation Example 2 of porous silica: silica (average particle size 780 nm, specific surface area 158 m 2 / g) preparation:

[0066] The steps are basically the same as those in Example 1 for preparing silicon dioxide, except that in step (1), the speed of the sand mill is 6000 rpm and the grinding time is 40 min.

[0067] Preparation Example 3 of Porous Silica: Silica (average particle size 410 nm, specific surface area 197 m 2 / g) preparation:

[0068] The steps are basically the same as those in Example 1 for preparing silicon dioxide, except that in step (1), the speed of the sand mill is 10,000 rpm and the grinding time is 60 min; and in step (2), the product is calcined at 600° C. for 5 h.

[0069] Preparation Example 4 of porous silica: silica (average particle size 190 nm, specific surface area 219 m 2 / g) preparation:

[0070] The steps are basically the same as those in Example 1 for preparing silicon dioxide, except that in step (1), the speed of the sand mill is 10,000 rpm and the grinding time is 70 min; and in step (6), the product is calcined at 600° C. for 4.5 h.

[0071] Preparation Example 5 of Porous Silica: Preparation of Silica (average particle size of 980 nm, specific surface area of ​​68 m2 / g):

[0072] The steps are basically the same as those in Example 1 for preparing silicon dioxide, except that in step (1), the speed of the sand mill is 2000 rpm and the grinding time is 20 min.

[0073] The guar gum used in this application is the building material grade guar gum produced by Beijing Guar Run Technology Co., Ltd.

[0074] The perfluorohexanone microcapsule fire extinguishing media prepared in Examples 4-6 and Comparative Examples 1-6 were made into fire extinguishing patches, and the fire extinguishing performance and storage stability of the prepared fire extinguishing patches were tested.

[0075] The preparation method of the fire extinguishing patch is as follows: 80g of microcapsules are added to 76g of water-soluble melamine-formaldehyde resin, stirred for 10 minutes, poured into a mold, and dried at 40°C to obtain a perfluorohexanone fire extinguishing patch (size: 34mm×24mm×3mm); a layer of polydimethylsiloxane of about 50μm is scraped on the surface of the fire extinguishing patch, a layer of double-sided tape is covered on the back of the fire extinguishing patch, and then a layer of iron sheet is covered, and a round magnet is attracted to the iron sheet to make a perfluorohexanone microcapsule fire extinguishing patch.

[0076] The method of fire extinguishing performance test is as follows: use 800℃ flame as the fire source, measure the temperature with an infrared thermometer, measure the fire extinguishing time with a stopwatch, fix the fire extinguishing patch on the surface of the stamped steel plate, and place the sheet downward at 1.5cm outside the flame. Measure the fire extinguishing time and the temperature difference before and after the fire extinguishing on the upper part of the sheet. Use the fire extinguishing time and temperature difference to characterize the fire extinguishing performance.

[0077] Storage stability test of perfluorohexanone microcapsule fire extinguishing medium: Place 100g of perfluorohexanone microcapsule fire extinguishing medium in an 80°C oven and dry for 12 hours, and calculate the weight retention rate of the perfluorohexanone microcapsule fire extinguishing medium.

[0078] The test results of fire extinguishing performance and storage stability are shown in Table 1.

[0079] Table 1

[0080]

[0081]

[0082] It can be seen from Table 1 that the fire extinguishing patch prepared by the perfluorohexanone microcapsule fire extinguishing medium of Examples 5-6 of the present application has a fire extinguishing time of less than 6s. During the stability test, the weight retention rate of the perfluorohexanone microcapsule fire extinguishing medium reaches more than 96.5%.

[0083] Comparative Example 1 and Comparative Example 2 are comparative examples in which the modified guar gum is replaced by guar gum and diphenylphosphine chloride and unmodified guar gum, respectively. As can be seen from Table 1, the fire extinguishing time is greater than 8.5 s.

[0084] Comparative Example 3 is a comparative example in which the modified guar gum is replaced by modified chitosan. As can be seen from Table 1, the fire extinguishing time is 8.6 s.

[0085] Comparative Examples 4 and 5 are comparative examples using silicon dioxide with different particle sizes. It can be seen from Table 1 that the fire extinguishing time is greater than 9s.

[0086] Comparative Example 6 is a perfluorohexanone microcapsule fire extinguishing medium prepared by the method of Example 2 of Chinese invention patent publication number CN 116271675 A. During the stability test, the weight retention rate of the perfluorohexanone microcapsule fire extinguishing medium was only 92.3%, and its storage stability was poor.

[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A perfluorohexanone microcapsule fire extinguishing medium, consisting of a core material and a shell material, It is characterized in that The core material includes perfluorohexanone, silicon dioxide, and azobisisobutyronitrile, and the shell material includes modified guar gum, acrylic resin, aluminum hydroxide, potassium nitrate, and an emulsifier; The modified guar gum is prepared by the following method: Tetrahydrofuran, guar gum and triethylamine are added to the reactor in sequence, stirred and mixed, and then a tetrahydrofuran solution of diphenylphosphinyl chloride is added dropwise. After the addition is completed, the temperature is raised to 75-85° C. and reacted for 10-14 hours. After post-treatment, guar gum modified with diphenylphosphinyl chloride is obtained.

2. A perfluorohexanone microcapsule fire extinguishing medium according to claim 1, It is characterized in that The mass ratio of the guar gum, triethylamine and diphenylphosphine chloride is 100:(10-15):(15-20).

3. A perfluorohexanone microcapsule fire extinguishing medium according to claim 1, It is characterized in that The silicon dioxide is porous silicon dioxide with an average particle size of 400-800nm ​​and a specific surface area of ​​150-200m 2 / g.

4. A perfluorohexanone microcapsule fire extinguishing medium according to claim 1, It is characterized in that The mass ratio of perfluorohexanone, silicon dioxide and azobisisobutyronitrile is 10:(2-3):(0.04-0.06).

5. A perfluorohexanone microcapsule fire extinguishing medium according to claim 1, It is characterized in that The mass ratio of the modified guar gum, acrylic resin, aluminum hydroxide, potassium nitrate and emulsifier is 100:(6-10):(12-18):(1-2):(8-10).

6. A perfluorohexanone microcapsule fire extinguishing medium according to claim 1, It is characterized in that The emulsifier is one of SR-20 and ER-10.

7. A process for preparing the perfluorohexanone microcapsule fire extinguishing medium according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1: adding perfluorohexanone, silicon dioxide and azobisisobutyronitrile into a reactor, stirring and mixing them thoroughly to obtain a perfluorohexanone fire extinguishing mixed liquid; S2: adding deionized water, modified guar gum and potassium nitrate into a reactor, stirring and mixing, and obtaining an aqueous solution of modified guar gum; S3: slowly adding the perfluorohexanone fire extinguishing mixed liquid, acrylic resin and emulsifier into the aqueous solution of modified guar gum, and stirring to obtain an emulsion; S4: Add aluminum hydroxide to the emulsion, stir and mix, let stand for 2-6 hours, filter, wash with water, and freeze-dry to obtain perfluorohexanone microcapsule fire extinguishing medium.

Citation Information

Patent Citations

  • Perfluorohexanone microcapsule fire extinguishing medium and preparation method thereof

    CN116271675A

  • Flame-retardant fibers, flame-retardant paper and preparation method of flame-retardant paper

    CN111608001A

  • Perfluorohexanone microcapsule fire extinguishing material and preparation method thereof

    CN114748830A

  • Modified guar gum and preparation method thereof

    CN114751998A

  • Perfluorohexanone microcapsule fire extinguishing material and preparation method thereof

    US20230405381A1

Cited By

  • Multi-component gas fire extinguishing agent composition, capsule-based flexible fire extinguishing patch and preparation method

    CN119838184A

  • A multi-component gaseous fire extinguishing agent composition, a capsule-based flexible fire extinguishing patch and a method of manufacture

    CN119838184B

  • Heptafluoropropane fire extinguishing agent and preparation method thereof

    CN120586339A

  • Fire extinguishing medium and application thereof in electric energy metering device

    CN120966492A