Halogen-free flame-retardant polyurethane foaming composition and application thereof

By introducing phosphate structures and using viscosity-reducing agents in polycarbonate diols, combined with the synergistic effect of diisocyanate, the problems of flammability of polyurethane materials and excessive addition of flame retardants are solved, and high-performance halogen-free resistance is achieved Burn polyurethane foaming material.

CN118955851AActive Publication Date: 2024-11-15ZHEJIANG UNIV +1

Patent Information

Application Number
CN202411196806.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing polyurethane materials are flammable and have insufficient flame retardant performance, which leads to fire risks and safety threats. At the same time, excessive addition of flame retardant will reduce mechanical properties and affect foam uniformity.

Method used

A special phosphorus-containing chain transfer agent is used to introduce a phosphate structure into the polycarbonate diol, and it works in concert with diisocyanate, combining a viscosity-reducing agent to improve flame retardant performance and reduce viscosity, and achieve room temperature foaming and high mechanical properties. Halogen-free flame-retardant polyurethane foaming composition.

Benefits of technology

It achieves excellent flame retardant properties of halogen-free flame retardant polyurethane, high foaming rate, uniform bubble cells, soft and fine, and has high flame retardant properties and excellent mechanical properties to meet the needs of high-performance polyurethane materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955851A_ABST
    Figure CN118955851A_ABST
Patent Text Reader

Abstract

The invention discloses a halogen-free flame-retardant polyurethane foaming composition, which is prepared from the following raw materials in parts by weight: 30 to 70 parts of flame-retardant polycarbonate diol; 30 to 70 parts of polyether polyol; 45 to 65 parts of diisocyanate; 1 to 5 parts of small molecular polyol; 2-10 parts of a viscosity reducer; 1-5 parts of a processing aid; and 1-15 parts of a foaming aid. The preparation of the flame-retardant polycarbonate diol comprises the following steps: adding a catalyst, an epoxy compound and polyhydroxyalkyl phosphate into a high-pressure reactor, introducing CO2 into the high-pressure reactor, and polymerizing to obtain the flame-retardant polycarbonate diol. The halogen-free flame-retardant polyurethane foaming composition disclosed by the invention can be foamed at room temperature, and the prepared halogen-free flame-retardant foaming polyurethane has excellent flame retardancy, high foaming rate, uniform, soft and fine pores, high flame retardancy and excellent mechanical properties, and can meet the requirements of practical application or the field of high-performance polyurethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane, and particularly relates to a halogen-free flame-retardant polyurethane foaming composition and a preparation method of the halogen-free flame-retardant polyurethane foaming composition. Background Art

[0002] As a high-performance polymer material, polyurethane is widely used in the fields of construction, automobiles, and electronic appliances. Polyurethane foam has good thermal insulation properties and is often used in the construction industry as a thermal insulation material. Polyurethane elastomers have high strength and wear resistance and are widely used in the manufacture of tires and seals, which can improve the safety and ride comfort of vehicles. Secondly, polyurethane materials are used as key components such as electrical insulating paints and wire and cable protective covers due to their good insulation properties, ensuring the stable operation of electronic equipment. Among them, polyether polyols and polyester polyols are the two core raw materials for the production of polyurethane materials. Polyether polyols are known for their flexibility and provide excellent elasticity and softness for polyurethane products. They are especially suitable for application scenarios that require good resilience and low-temperature flexibility, such as soft furniture such as cushions and mattresses, but their overly soft characteristics sometimes limit their application in areas that require higher strength or hardness. In contrast, polyester polyols give polyurethane stronger hardness and better mechanical properties, making products made of polyester polyurethane, such as tires and hard foams, have excellent wear resistance and load-bearing capacity. However, the hardness of polyester polyurethane materials is too large and their water resistance is relatively poor. At the same time, both are not flame retardant and are even flammable.

[0003] The flammability of polyurethane materials is accompanied by fire risks. They burn quickly and release toxic gases, posing a threat to personnel safety and the environment. Improving flame retardancy not only enhances the safety of polyurethane materials, but also promotes their wide application in many fields, meeting the market demand for high-performance materials. With the increasing application of flame-retardant polyurethane materials, how to improve the flame retardancy of polyurethane materials has become the key. By adding flame retardants, its burning speed and heat release can be effectively reduced, and its flame retardant properties can be improved. However, this method usually requires the addition of more flame retardants. For example, a Chinese patent document with application publication number CN104861144A discloses a flame retardant rigid foam polyurethane, which is composed of the following components in parts by weight: 80-100 parts of polyether polyol, 2-4 parts of foaming agent, 10-30 parts of cross-linking agent, 1-3 parts of tertiary amine catalyst, 20-40 parts of compound flame retardant, and isocyanate index 1.0-2.5. In this technical solution, the flame retardant effect of the polyurethane rigid foam material is achieved by adding 20-40 parts of a composite flame retardant composed of a nitrogen-phosphorus expansion flame retardant and expanded vermiculite. However, the large amount of flame retardant added will reduce the mechanical properties of the polyurethane, such as the tensile strength and elongation at break, and will also cause the fluidity of the foam to deteriorate during the foaming process, thereby affecting the uniformity of the foaming and the molding quality.

[0004] The polyurethane foam material prepared from polycarbonate polyols has thermal insulation, sound absorption and noise reduction, and corrosion resistance comparable to other conventional polyester polyurethane foam materials, and has better mechanical properties and hydrolysis resistance. At the same time, the carbon dioxide-based polyol itself contains a certain mass fraction of CO2 (existing in a carbonate structure), and therefore has a certain flame retardancy, and is expected to be used to prepare flame-retardant polyurethane. Although carbon dioxide-based polyol products have entered the market and are used in coatings, adhesives and other fields, their high viscosity when used in polyurethane foam materials leads to problems such as difficulty in foaming operation. This limits its use in specific application areas, such as cold chain, building materials, coal mining plugging materials, and other occasions that have high requirements for flame retardancy and mechanical properties. Summary of the invention

[0005] In view of the above problems, the present invention discloses a halogen-free flame retardant polyurethane foam composition, which can be foamed at room temperature. The prepared halogen-free flame retardant polyurethane foam has excellent flame retardancy, high foaming rate, uniform, soft and dense foam cells, and both high flame retardancy and excellent mechanical properties, which can meet the needs of practical applications or high-performance polyurethane fields.

[0006] The specific technical solutions are as follows:

[0007] A halogen-free flame-retardant polyurethane foam composition, comprising, by weight, the following raw materials:

[0008]

[0009] The preparation of the flame retardant polycarbonate diol comprises:

[0010] Adding a catalyst, an epoxy compound, and a polyhydroxyalkyl phosphate into a high-pressure reactor, introducing CO2 into the high-pressure reactor, and preparing a flame-retardant polycarbonate diol after polymerization;

[0011] The viscosity reducer is selected from one or more of dimethyl (1-hydroxyethyl)phosphonate, diethyl hydroxymethylphosphonate, and dimethyl 2-hydroxyethylphosphonate.

[0012] The invention discloses a halogen-free flame-retardant polyurethane foaming composition. A phosphate structure is introduced into a polycarbonate diol main chain by adopting a special phosphorus-containing chain transfer agent, and a polycarbonate diol with excellent flame retardant performance is prepared in situ; the polycarbonate diol can also synergize with the nitrogen element in diisocyanate to further improve the flame retardant effect; the invention also adopts a special viscosity reducer, which significantly reduces the viscosity of the flame-retardant polycarbonate diol when added in a small amount, thereby improving the operation of the composition during application, so that the composition formula ingredients can be stirred at room temperature, and the prepared foamed polyurethane has a high foaming rate, uniform, soft and dense foam cells, and has both high flame retardancy and excellent mechanical properties by adjusting the composition formula.

[0013] The inventors speculate that the viscosity reducer used in the present invention can effectively reduce the intermolecular forces of the flame retardant polycarbonate diol and thus reduce the viscosity, similar to a plasticizer, but has a significant effect of reducing the viscosity of the polycarbonate diol system. However, it was found in the experiment that if conventional plasticizers such as dioctyl phthalate, dibutyl phthalate, dioctyl phthalate, dipropylene glycol dibenzoate, etc. are used at room temperature, the system viscosity is reduced to half to one third of the viscosity before adding the plasticizer. When a moderate amount of the viscosity reducer of the present invention is used, the system viscosity can be reduced to one tenth of the system viscosity or even lower.

[0014] In the present invention, when preparing the flame retardant polycarbonate diol:

[0015] The epoxy compound is selected from propylene oxide and / or butylene oxide;

[0016] The catalyst is selected from a zinc-cobalt double metal cyanide catalyst or a supported zinc-cobalt double metal cyanide catalyst; the mass proportion of the catalyst is 0.01 to 0.50 wt % based on the total mass of the epoxy compound;

[0017] The polyhydroxyalkyl phosphate is selected from phosphate molecules containing two or more hydroxyl groups, specifically selected from diethyl N,N-bis(2-hydroxyethyl)aminomethylenephosphonate, dihydroxyethyl bishydroxymethyl phosphate, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and one or more phosphorus-containing bisphenol compounds having the following structural formulas (1) to (4);

[0018]

[0019] In the present invention, polyhydroxyalkyl phosphate is used as a chain transfer agent to prepare flame-retardant polycarbonate diol. Experiments have shown that during the chain transfer polymerization process, it enters the main chain by rapid chain transfer and is located in the middle of the main chain, which can significantly increase the flame retardancy of the polycarbonate diol to UL 94V0 level.

[0020] Based on the total mass of the epoxy compound, the mass proportion of the polyhydroxyalkyl phosphate is 0.5 to 1.5 wt %.

[0021] CO2 is introduced into the high-pressure reactor until the pressure reaches 1-5 MPa and the polymerization reaction temperature reaches 50-100°C.

[0022] The crude product obtained after polymerization needs to be washed, filtered, dried, purified and impurities removed.

[0023] Preferred:

[0024] The preparation of the flame retardant polycarbonate diol comprises:

[0025] (1) adding a catalyst, an epoxy compound, and a polyhydroxyalkyl phosphate into a high-pressure reactor, introducing CO2 into the high-pressure reactor, and then performing a bulk polymerization and then performing a pressure relief and vacuum treatment;

[0026] (2) Under the protection of nitrogen at normal pressure, ethylene oxide and a solvent are added into a high-pressure reactor to obtain a flame-retardant polycarbonate ether polyol after reaction.

[0027] It has been found through experiments that ethylene oxide can be introduced into the end of the polyol molecular chain, so that the hydroxyl group at the end of the polyol is converted into a primary hydroxyl group, thereby increasing the reactivity of the polyol with isocyanate, which is beneficial to the foaming effect of the polyurethane material. However, the polyurethane prepared by the flame-retardant polycarbonate diol that has not been treated in step (2) has a poor foaming effect, a long foaming time, and slightly reduced mechanical properties.

[0028] In step (2):

[0029] Based on the total mass of the epoxy compound, the mass proportion of ethylene oxide is generally 5-10wt%;

[0030] The solvent is selected from one or more of dimethyl carbonate, tetrahydrofuran, dichloromethane and chloroform;

[0031] Based on the total mass of the epoxy compound, the mass proportion of the solvent is generally 30-40wt% of the epoxy compound;

[0032] The reaction temperature is 50-100°C.

[0033] The crude product obtained after the reaction in step (2) needs to be washed, filtered, dried, purified and impurities removed.

[0034] The halogen-free flame-retardant polyurethane foam composition disclosed in the present invention:

[0035] The polyether polyol is selected from conventional types in the art, including but not limited to one or more of polyoxypropylene diol, polyoxyethylene diol, polytetrahydrofuran diol, tetrahydrofuran-oxypropylene copolymer diol, and polyoxypropylene triol; the molecular weight is 400 to 2000 g / mol. The use of polyether polyol can improve the hardness of carbon dioxide-based polyol when used to prepare polyurethane foam materials, improve the flexibility of the molecular chain, and improve the flexibility, mechanical properties and impact resistance of the material through cross-linking. The amount of polyether polyol introduced is adjusted according to the performance of the final product.

[0036] The diisocyanate is selected from conventional types in the art, including but not limited to one or more of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), naphthalene 1,5-diisocyanate (NDI), trans-1,4-cyclohexyl diisocyanate (CHDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), isophorone diisocyanate (IPDI), and p-phenylene diisocyanate (PPDI); isocyanates containing a benzene ring structure are often preferred, and liquefiable mixed isocyanates are particularly preferred, and their usage is calculated according to the hydroxyl value of the composition.

[0037] Due to containing benzene ring rigid group, relatively stable structure can be maintained at high temperature, not easy to thermally decompose or burn, help to slow down the thermal degradation rate of material, reduce the release amount of combustible gas, thus improve the flame retardant property of material. Meanwhile, in the combustion process, isocyanate containing benzene ring may form carbon layer by complex chemical reaction, is a kind of poor conductor of heat, can isolate the transfer of heat and oxygen, thus slow down the burning rate of material. And isocyanate may decompose and produce some incombustible or difficult to burn gas (such as nitrogen, carbon dioxide etc.) at high temperature, can dilute the concentration of combustible gas, reduce the speed and intensity of combustion reaction. The present invention designs phosphorus-containing polycarbonate diol, also is based on the consideration of diisocyanate nitrogen-containing element, thus can directly utilize the synergistic effect of phosphorus and nitrogen in flame retardant process. Due to the presence of phosphate, phosphoric acid is formed after its thermal decomposition, thereby is conducive to the carbonization of whole material.

[0038] The small molecule polyol is selected from conventional types in the art, including but not limited to one or more of glycerol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-octanediol, 3-methyl-1-butanol, neopentyl glycol, triethylene glycol, trimethylolpropane, sorbitol, and pentaerythritol; small molecule polyols can be used to adjust the hardness and strength of the foaming material, and also have a significant effect on the elasticity and modulus of the polyurethane foaming material. During the foaming process, the reaction rate of the small molecule polyol and the isocyanate will affect the uniformity and stability of the foaming. The appropriate reaction rate can ensure that the foaming material has a uniform pore structure and good physical properties. In addition, the small molecule polyol may also indirectly affect the foaming process by affecting parameters such as the viscosity of the reaction system.

[0039] The processing aids include antioxidants and / or ultraviolet absorbers.

[0040] The antioxidant is selected from conventional types in the art, including but not limited to one or more of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate), and tris(2,4-di-tert-butylphenyl) phosphite. Antioxidants delay or inhibit the oxidation process of the polymer, thereby preventing the aging of the polyurethane and extending its service life, preventing scorching during the foaming process, and inhibiting the occurrence of high-temperature yellowing.

[0041] The ultraviolet absorber is selected from conventional types in the art, including but not limited to one or more of bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, 2-hydroxy-4-n-octyloxybenzophenone, 4-methoxy-2-hydroxybenzophenone, 2-(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol, and phenyl o-hydroxybenzoate. Organic polymer materials containing unsaturated chromogenic functional groups can absorb ultraviolet radiation under sunlight irradiation. When the absorbed energy exceeds its bond energy, it can cause chemical bond breakage and accelerate the oxidative degradation of the material, thereby causing material damage and failure. The introduction of ultraviolet absorbers can effectively slow down the ultraviolet aging of biodegradable fibers.

[0042] The foaming aid comprises a foaming agent, a catalyst and silicone oil;

[0043] The foaming agent is selected from one or more of water, cyclopentane, dichloromethane, azodicarbonamide, etc.;

[0044] The catalyst is selected from one or more of dibutyltin dilaurate, triethylenediamine, bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine, and pentamethyldiethylenetriamine;

[0045] The mass ratio of the foaming agent, the catalyst and the silicone oil is (3-15):1:(1-5).

[0046] Based on the above preferred raw materials, further preferred are:

[0047] The halogen-free flame-retardant polyurethane foam composition comprises, by weight, the following raw materials:

[0048]

[0049]

[0050] The present invention also discloses a method for preparing a halogen-free flame-retardant polyurethane foam, wherein the raw materials are mixed uniformly at room temperature according to their respective weight parts and then foamed. The preparation method is simple and controllable, and can be industrially scaled up and applied in practice.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] 1. In the halogen-free flame-retardant foaming polyurethane composition provided by the present invention, its phosphate structure enters the main chain of the polycarbonate diol through a rapid chain transfer polymerization reaction, and is a macromolecular flame retardant. Compared with the traditional KOH method polyether polyol preparation of polyurethane using an ester exchange method under high temperature conditions, the phosphate diol is easily decomposed, and it is impossible or difficult to introduce the phosphate structure into the main chain of the molecule. At the same time, the present invention also overcomes the shortcomings of the flame retardant performance of the traditional ester exchange method polycarbonate polyol, adopts the CO2 bulk polymerization method, and strengthens the flame retardant performance of the material obtained by the reaction of carbon dioxide-based polyols and isocyanates. Due to the presence of phosphorus, the carbamate bond that can be formed can improve the flame retardant performance of the product through phosphorus-nitrogen synergy, and can meet the use requirements of applications with flame retardant requirements with significantly less or no additional polymerization inhibitor.

[0053] 2. The halogen-free flame-retardant foaming polyurethane composition provided by the present invention overcomes the problem of high viscosity and difficult construction when carbon dioxide-based polyols are used in polyurethane materials. By introducing a small amount of special phosphorus-containing viscosity reducer, the viscosity of the composition during operation is significantly reduced, so that the composition can be stirred and operated at room temperature according to the formula ingredients, and is easy to foam; at the same time, it can also further play a good flame retardant role.

[0054] 3. The halogen-free flame-retardant polyurethane foam composition provided by the present invention has low production cost, and many raw materials thereof are commercially available raw materials, and the flame-retardant polycarbonate diol can also be produced at low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 is the stress-strain curve of the flame retardant polyurethane foam material prepared in Example 1;

[0056] Figure 2 This is a photo of the flame retardant polyurethane foam prepared in Example 1. DETAILED DESCRIPTION

[0057] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.

[0058] Unless otherwise specified, the raw materials in all the examples and comparative examples of the present invention were purchased through commercial channels.

[0059] Example 1

[0060] Step 1: Add 0.2g zinc-cobalt double metal cyanide catalyst, 10g N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester, and 1200g propylene oxide into a dry high-pressure reactor, introduce CO2 at a temperature of 100°C until the pressure in the reactor is 5MPa, and perform bulk polymerization for 8h, then remove the propylene oxide in the crude product by depressurization and vacuum, and then add 20g ethylene oxide and 500g tetrahydrofuran to the reactor under the protection of nitrogen at normal pressure. After the dissolved viscosity decreases, continue to react at a temperature of 80°C for 6h and then cool. After purifying and refining the crude product, the final product, flame-retardant polycarbonate diol, is obtained.

[0061] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3500 g / mol, and the molecular weight distribution was 1.5.

[0062] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 30wt%, and the hydroxyl value was 35mgKOH / g.

[0063] Step 2: 30 parts of the flame-retardant polycarbonate diol prepared in step 1 (unless otherwise specified, all raw materials in the present invention are measured in parts by weight), 70 parts of polyoxypropylene diol, 60 parts of diphenylmethane diisocyanate, 7 parts of (1-hydroxyethyl) dimethyl phosphonate, 3 parts of propylene glycol, 1 part of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1 part of bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, 1 part of dibutyltin dilaurate, 1 part of silicone oil and 8 parts of water are mixed evenly and foamed after high-speed stirring for 20 seconds.

[0064] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores.

[0065] Example 2

[0066] The preparation process is basically the same as that in Example 1, except that:

[0067] The amount of the flame retardant polycarbonate diol in step 2 is replaced with 40 parts, and the amount of the polyether polyol is replaced with 60 parts.

[0068] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores.

[0069] Example 3

[0070] The preparation process is basically the same as that in Example 1, except that:

[0071] The amount of the flame retardant polycarbonate diol in step 2 is replaced with 50 parts, and the amount of the polyether polyol is replaced with 50 parts.

[0072] The flame-retardant foamed polyurethane prepared in this embodiment has poor elasticity and is relatively hard.

[0073] Example 4

[0074] The preparation process is basically the same as that in Example 1, except that:

[0075] The amount of the flame retardant polycarbonate diol in step 2 is replaced with 60 parts, and the amount of the polyether polyol is replaced with 40 parts.

[0076] The flame-retardant foamed polyurethane prepared in this embodiment has poor elasticity and is relatively hard.

[0077] Example 5

[0078] The preparation process is basically the same as that in Example 1, except that:

[0079] The amount of the flame retardant polycarbonate diol in step 2 is replaced with 70 parts, and the amount of the polyether polyol is replaced with 30 parts.

[0080] The flame-retardant foamed polyurethane prepared in this embodiment has poor elasticity and is relatively hard.

[0081] Example 6

[0082] Step 1: Add 0.2g zinc-cobalt double metal cyanide catalyst, 10g N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester, and 1200g propylene oxide into a dry high-pressure reactor, introduce CO2 at a temperature of 80°C until the pressure in the reactor is 4MPa, and perform bulk polymerization for 6h, then remove the propylene oxide in the crude product by depressurization and vacuum, and then add 20g ethylene oxide and 500g tetrahydrofuran to the reactor under the protection of nitrogen at normal pressure. After the dissolved viscosity decreases, continue to react at a temperature of 80°C for 6h and then cool. After purifying and refining the crude product, the final product, flame-retardant polycarbonate diol, is obtained.

[0083] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3000 g / mol, and the molecular weight distribution was 1.8.

[0084] through 1 H NMR test showed that the mass fraction of CO2 in the flame retardant polycarbonate diol was 20wt% and the hydroxyl value was 30mgKOH / g.

[0085] Step 2: Mix 30 parts of the flame-retardant polycarbonate diol prepared in step 1, 70 parts of polyoxypropylene diol, 60 parts of diphenylmethane diisocyanate, 7 parts of (1-hydroxyethyl) dimethyl phosphonate, 3 parts of propylene glycol, 1 part of octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1 part of bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, 1 part of dibutyltin dilaurate, 1 part of silicone oil and 8 parts of water, and stir at high speed for 20 seconds before foaming.

[0086] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0087] Example 7

[0088] The preparation process is basically the same as that in Example 6, except that:

[0089] The amount of diphenylmethane diisocyanate in step 2 is replaced with 45 parts.

[0090] The flame retardant foamed polyurethane prepared in this embodiment has a poor foaming effect.

[0091] Example 8

[0092] The preparation process is basically the same as that in Example 6, except that:

[0093] The amount of diphenylmethane diisocyanate in step 2 was replaced with 55 parts.

[0094] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores.

[0095] Example 9

[0096] The preparation process is basically the same as that in Example 1, except that:

[0097] The amount of (1-hydroxyethyl)phosphonic acid dimethyl ester in step 2 was replaced by 2 parts.

[0098] The flame-retardant polyurethane foam prepared in this embodiment is non-uniformly foamed.

[0099] Example 10

[0100] The preparation process is basically the same as that in Example 1, except that:

[0101] The amount of dimethyl (1-hydroxyethyl)phosphonate in step 2 was replaced with 4 parts.

[0102] The flame-retardant polyurethane foam prepared in this embodiment is non-uniformly foamed.

[0103] Embodiment 11

[0104] The preparation process is basically the same as that in Example 1, except that:

[0105] The amount of (1-hydroxyethyl)phosphonic acid dimethyl ester in step 2 was replaced with 6 parts.

[0106] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Embodiment 1.

[0107] Example 12

[0108] The preparation process is basically the same as that in Example 1, except that:

[0109] The amount of (1-hydroxyethyl)phosphonic acid dimethyl ester in step 2 is replaced by 10 parts.

[0110] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Embodiment 1.

[0111] Example 13

[0112] The preparation process is basically the same as that in Example 1, except that:

[0113] The N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester in step 1 was replaced with an equal mass of dihydroxyethyl bishydroxymethyl phosphate.

[0114] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3200 g / mol, and the molecular weight distribution was 1.4.

[0115] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 32wt%, and the hydroxyl value was 38mgKOH / g.

[0116] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0117] Embodiment 14

[0118] The preparation process is basically the same as that in Example 1, except that:

[0119] The N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester in step 1 is replaced with an equal mass of a phosphorus-containing bisphenol compound (structural formula 1).

[0120] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3800 g / mol, and the molecular weight distribution was 1.8.

[0121] through 1H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 28wt% and the hydroxyl value was 33mgKOH / g.

[0122] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0123] Embodiment 15

[0124] The preparation process is basically the same as that in Example 1, except that:

[0125] The N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester in step 1 is replaced with an equal mass of a phosphorus-containing bisphenol compound (structural formula 2).

[0126] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3700 g / mol, and the molecular weight distribution was 1.7.

[0127] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 29wt% and the hydroxyl value was 34mgKOH / g.

[0128] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0129] Example 16

[0130] The preparation process is basically the same as that in Example 1, except that:

[0131] The N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester in step 1 is replaced with an equal mass of a phosphorus-containing bisphenol compound (structural formula 3).

[0132] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3800 g / mol, and the molecular weight distribution was 1.8.

[0133] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 28wt% and the hydroxyl value was 33mgKOH / g.

[0134] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0135] Embodiment 17

[0136] The preparation process is basically the same as that in Example 1, except that:

[0137] The N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester in step 1 is replaced with an equal mass of a phosphorus-containing bisphenol compound (structural formula 4).

[0138] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3900 g / mol, and the molecular weight distribution was 1.9.

[0139] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 28wt% and the hydroxyl value was 33mgKOH / g.

[0140] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0141] Embodiment 18

[0142] The preparation process is basically the same as that in Example 1, except that:

[0143] The (1-hydroxyethyl)phosphonic acid dimethyl ester in step 2 is replaced by an equal mass of hydroxymethylphosphonic acid diethyl ester.

[0144] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0145] Embodiment 19

[0146] The preparation process is basically the same as that in Example 1, except that:

[0147] The (1-hydroxyethyl)phosphonic acid dimethyl ester in step 2 is replaced by an equal mass of 2-hydroxyethylphosphonic acid dimethyl ester.

[0148] The flame-retardant polyurethane foam prepared in this embodiment has uniform, soft and dense pores, similar to those in Example 1.

[0149] Embodiment 20

[0150] The preparation process is basically the same as that in Example 1, except that:

[0151] In step 1, 0.2 g of zinc-cobalt double metal cyanide catalyst, 10 g of N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester, and 1200 g of propylene oxide are added to a dry high-pressure reactor, and CO2 is introduced at a temperature of 100° C. until the pressure in the reactor is 5 MPa. After bulk polymerization for 8 hours, polycarbonate diol is obtained, and the propylene oxide in the crude product is removed by depressurization and vacuum, and then the product is directly washed, filtered, dried, purified, and impurities are removed.

[0152] The molecular weight of the flame-retardant polycarbonate diol prepared in step 1 was determined by gel chromatography to be 3500 g / mol, and the molecular weight distribution was 1.5.

[0153] through 1 H NMR test showed that the CO2 mass fraction in the flame retardant polycarbonate diol was 30wt%, and the hydroxyl value was 20mgKOH / g.

[0154] The flame retardant polyurethane foam prepared in this example has a poorer foaming effect than that in Example 1.

[0155] Comparative Example 1

[0156] The preparation process is basically the same as that in Example 1, except that:

[0157] In step (1), when preparing the polymer, no N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester is added to prepare the polycarbonate diol.

[0158] The foamed polyurethane prepared in this comparative example has uniform, soft and dense pores.

[0159] Comparative Example 2

[0160] The preparation process is basically the same as that in Example 1, except that:

[0161] In step 2, no (1-hydroxyethyl)phosphonic acid dimethyl ester was added.

[0162] The foamed polyurethane prepared in this comparative example is not foamed uniformly.

[0163] Comparative Example 3

[0164] The preparation process is basically the same as that in Example 1, except that:

[0165] In step 2, dimethyl (1-hydroxyethyl)phosphonate is replaced with an equal mass of dioctyl phthalate.

[0166] The foamed polyurethane prepared in this comparative example foams unevenly and has a poor effect.

[0167] Comparative Example 4

[0168] The preparation process is basically the same as that in Comparative Example 1, except that:

[0169] In step 2, the mass of dimethyl (1-hydroxyethyl)phosphonate is replaced with 30 parts.

[0170] The foamed polyurethane prepared in this comparative example foams unevenly and has a poor effect.

[0171] Comparative Example 5

[0172] The preparation process is basically the same as that in Example 1, except that:

[0173] The amount of diphenylmethane diisocyanate in step 2 is replaced with 25 parts.

[0174] The foamed polyurethane prepared in this comparative example failed to foam.

[0175] Comparative Example 6

[0176] The preparation process is basically the same as that in Example 1, except that:

[0177] The amount of diphenylmethane diisocyanate in step 2 is replaced with 35 parts.

[0178] The foamed polyurethane prepared in this comparative example failed to foam.

[0179] Performance Testing:

[0180] The foaming conditions, flame retardant properties (GB / T26700-2011), and mechanical properties (GB / T 9641) of the foamed polyurethanes prepared in each embodiment and each comparative example are listed in the following Table 1.

[0181] Table 1

[0182]

[0183]

[0184] The above-mentioned embodiments are preferred embodiments, but the protection scope of the present invention is not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above-mentioned embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.

Claims

1. A halogen-free flame-retardant polyurethane foam composition, characterized in that: By weight, the raw material composition includes: The preparation of the flame retardant polycarbonate diol comprises: Adding a catalyst, an epoxy compound, and a polyhydroxyalkyl phosphate into a high-pressure reactor, introducing CO2 into the high-pressure reactor, and preparing a flame-retardant polycarbonate diol after polymerization; The viscosity reducer is selected from one or more of dimethyl (1-hydroxyethyl)phosphonate, diethyl hydroxymethylphosphonate, and dimethyl 2-hydroxyethylphosphonate.

2. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: The catalyst is selected from zinc-cobalt double metal cyanide catalyst or supported zinc-cobalt double metal cyanide catalyst; The epoxy compound is selected from propylene oxide and / or butylene oxide; The polyhydroxyalkyl phosphate is selected from phosphate molecules containing 2 or more hydroxyl groups; Based on the total mass of the epoxy compound, the mass proportion of the catalyst is 0.01-0.50 wt%, and the mass proportion of the polyhydroxyalkyl phosphate is 0.5-1.5 wt%.

3. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: Access The pressure in the CO2 high-pressure reactor is 1-5 MPa, and the polymerization reaction temperature is 50-100°C.

4. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: The polyether polyol is selected from one or more of polyoxypropylene diol, polyoxyethylene diol, polytetrahydrofuran diol, tetrahydrofuran-oxypropylene copolymer diol, and polyoxypropylene triol; The diisocyanate is selected from one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, naphthalene 1,5-diisocyanate, trans-1,4-cyclohexyl diisocyanate, 4,4′-dicyclohexylmethane diisocyanate, isophorone diisocyanate, and p-phenylene diisocyanate; The small molecule polyol is selected from one or more of glycerol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-octanediol, 3-methyl-1-butanol, neopentyl glycol, triethylene glycol, trimethylolpropane, sorbitol, and pentaerythritol; The processing aids include antioxidants and / or ultraviolet absorbers.

5. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: The foaming aid comprises a foaming agent, a catalyst and silicone oil; The foaming agent is selected from one or more of water, cyclopentane, dichloromethane, and azodicarbonamide; The catalyst is selected from one or more of dibutyltin dilaurate, triethylenediamine, bis(dimethylaminoethyl) ether, N,N-dimethylcyclohexylamine, and pentamethyldiethylenetriamine; The mass ratio of the foaming agent, the catalyst and the silicone oil is (3-15):1:(1-5).

6. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: The polyhydroxyalkyl phosphate is selected from one or more of N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester, dihydroxyethyl bishydroxymethyl phosphate, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide, and phosphorus-containing bisphenol compounds having the following structural formulas (1) to (4); 7. The halogen-free flame-retardant polyurethane foam composition according to claim 1, characterized in that: The preparation of the flame retardant polycarbonate diol comprises: (1) adding a catalyst, an epoxy compound, and a polyhydroxyalkyl phosphate into a high-pressure reactor, introducing CO2 into the high-pressure reactor, and then performing a bulk polymerization and then performing a pressure relief and vacuum treatment; (2) Under the protection of nitrogen at normal pressure, ethylene oxide and a solvent are added into a high-pressure reactor to obtain a flame-retardant polycarbonate ether polyol after reaction.

8. The halogen-free flame-retardant polyurethane foam composition according to claim 7, characterized in that: In step (2): Based on the total mass of the epoxy compound, the mass proportion of ethylene oxide is 5 to 10 wt%; The solvent is selected from one or more of dimethyl carbonate, tetrahydrofuran, dichloromethane and chloroform; Based on the total mass of the epoxy compound, the mass proportion of the solvent is 30-40wt% of the epoxy compound; The reaction temperature is 50-100°C.

9. A halogen-free flame-retardant polyurethane foam composition according to any one of claims 1 to 8, characterized in that: By weight, the raw material composition includes:

10. A method for preparing a halogen-free flame-retardant polyurethane foam, characterized in that: According to any one of claims 1 to 9, the halogen-free flame-retardant polyurethane foam composition is prepared by uniformly mixing the raw materials according to their respective mass parts at room temperature and then foaming them.

Citation Information

Patent Citations

  • Flame retardant hard bubble polyurethane

    CN104861144A

  • Novel polyurethane foaming material

    CN113717345A

  • Foamed polyurethane as well as preparation method and application thereof

    CN113980233A

  • Carbon dioxide-based flame-retardant bi-component polyurethane structure adhesive and preparation method thereof

    CN116218453A

  • Flame-retardant polyurethane flexible foam with excellent mechanical property and preparation method thereof

    CN116425938A

Cited By

  • Environment-friendly high-performance flame-retardant shock-absorbing impact-resistant composite material and preparation method thereof

    CN120005381A

  • High-stability foaming composition for polyurethane and application thereof

    CN120040954A

  • Phosphorus-containing compound, flame-retardant and heat-resistant composition, pre-preg, and metal-clad laminate

    TWI923543B