Lipoic acid (at) Cu-MOF material with pH and humidity dual response as well as preparation method and application thereof

By preparing lipoic acid @Cu-MOF material with dual pH and humidity response, Cu-MOF's shortcomings in the fields of antibacterial performance optimization and fruit and vegetable preservation are solved, high-effect vegetable preservation is achieved, and the shelf life of fruit and vegetable is extended and its quality is maintained.

CN118955938AActive Publication Date: 2024-11-15HEFEI UNIV OF TECH

Patent Information

Application Number
CN202411445813.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

The existing fruit and vegetable preservation technology is unreasonable in commercially, and Cu-MOF has insufficient research on the fields of antibacterial performance optimization and fruit and vegetable preservation, making it difficult to effectively extend the shelf life of fruit and vegetable and maintain their quality.

Method used

Using lipoic acid @Cu-MOF material with dual pH and humidity response, Cu-MOF crystals are prepared by reaction between copper source and organic ligand, and combined with lipoic acid to form a high load and tight coordination material, using sulfur The thiol group of the caprylic acid forms coordination bonds with the copper ions, enhancing the material's sensitivity to environmental changes and forming a fruit and vegetable preservation material with antioxidant and antibacterial effects.

Benefits of technology

It realizes the preparation of high-effect vegetable fresh preservation materials at low energy consumption and low cost. Lipoic acid @Cu-MOF material can control the release of lipoic acid according to changes in environmental pH and humidity, maximize the antioxidant and antibacterial effects, and make up for Cu-MOF in the anti-anti- Deficiencies in oxidation and antifungal properties extend the shelf life of fruits and vegetables and maintain their freshness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955938A_ABST
    Figure CN118955938A_ABST
Patent Text Reader

Abstract

The invention discloses a lipoic acid (at) Cu-MOF material with pH and humidity dual response as well as a preparation method and application of the lipoic acid (at) Cu-MOF material. The preparation method comprises the following steps: fully mixing a copper source solution and an organic ligand solution, reacting, washing, carrying out first drying treatment, soaking in dichloromethane, and carrying out vacuum drying treatment to obtain a Cu-MOF crystal; the preparation method comprises the following steps: dispersing Cu-MOF crystals in ethanol, mixing with a lipoic acid solution, carrying out ultrasonic treatment, adding water under a stirring condition, continuously reacting, washing, and carrying out vacuum drying treatment to prepare the lipoic acid-coated Cu-MOF material with pH and humidity dual responses. The preparation method provided by the invention is low in energy consumption, simple to operate and low in cost; meanwhile, the lipoic acid coated Cu-MOF material is high in loading capacity and tight in coordination, and release of lipoic acid can be controlled by responding to pH and humidity changes in the environment, so that the lipoic acid coated Cu-MOF material has a better application prospect in the field of fruit and vegetable preservation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fruit and vegetable storage and preservation materials, and relates to a lipoic acid@Cu-MOF material with dual response to pH and humidity, and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of science and technology, new fruit and vegetable preservation technologies have emerged, such as microbial treatment, radiation sterilization, vacuum packaging, membrane technology, biological preservatives, etc. At present, there are many experiments aimed at protecting fruits and vegetables from oxidation and enzymatic browning, such as low-temperature storage, controlled atmosphere refrigeration, mild preheating treatment, UV-A light treatment, xanthan gum plus cinnamic acid coating, chitosan coating, oil fumigation, melatonin treatment, rosemary extract and single oxygen pretreatment combined and post-harvest inoculation. However, some of these preservation methods are not commercially reasonable due to the need to verify effectiveness or low consumer preference. Therefore, the research and application of fruit and vegetable preservation technology has important theoretical and practical significance, and is of great significance for improving the market competitiveness of fruits and vegetables, reducing food waste, ensuring food safety and meeting people's demand for healthy diet.

[0003] Lipoic acid is a plant growth regulator with multiple functions such as antioxidant, anti-inflammatory and antibacterial, which can participate in the regulation of plant growth. It can affect plant development by scavenging reactive oxygen free radicals, regulating biological rhythms, and regulating the ripening and aging process of fruits. In recent years, lipoic acid treatment has been found to extend the storage and shelf life of post-harvest fruits and vegetables. It helps maintain the quality of fruits and vegetables, delays their aging process, and can achieve good preservation effects even at lower concentrations.

[0004] MOF is a type of crystalline material formed by metal ions or clusters connected to organic ligands through coordination bonds. It has the characteristics of high adjustability, pore structure and surface functionalization. Cu-MOF is formed by copper ions and organic ligands under specific conditions. It has good stability, controllable pore structure and surface active sites. Therefore, it has broad application prospects in gas adsorption, separation, catalysis and other fields. Due to its unique structure and properties, MOF materials have shown great application potential in environmental protection, drug delivery and molecular controlled release, and have received extensive attention and research. However, the research on Cu-MOF in the field of antibacterial performance optimization and fruit and vegetable preservation has not been studied yet.

[0005] Thin film technology has many advantages in preserving vegetables and fruits. It is convenient, economical and safe. It can extend the shelf life of products, maintain their quality and freshness, and meet consumers' demand for high-quality food. Among them, sodium alginate is a kind of alginate extracted from brown algae, which has high safety and gel properties. Due to its transparency and excellent mechanical properties, sodium alginate is widely used in the pharmaceutical and food industries. In recent years, sodium alginate has been widely used in the production of food cling film, which can provide excellent protection, prevent food from moisture and contamination, and extend the shelf life of food. At the same time, it also has good degradability and is environmentally friendly. In addition, the intelligent responsive controlled release system is an important area of ​​current research. It has the characteristics of being able to respond to external stimuli or changes. These stimuli can include factors such as pH, gas, temperature and humidity. The intelligent responsive controlled release system can release active substances at the optimal time and conditions. The application potential of the intelligent responsive controlled release system is wide, and it can bring important innovations and progress in the fields of medicine, agriculture and food. Summary of the invention

[0006] The main purpose of the present invention is to provide a lipoic acid@Cu-MOF material with dual response to pH and humidity and a preparation method and application thereof to overcome the shortcomings of the prior art.

[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: The embodiment of the present invention provides a method for preparing a lipoic acid@Cu-MOF material having dual responses to pH and humidity, which comprises: The copper source solution and the organic ligand solution are fully mixed and reacted at 120-150° C. for 12-15 hours, followed by washing and a first drying process, and then the obtained product is immersed in dichloromethane and subjected to vacuum drying to obtain Cu-MOF crystals; wherein the copper source solution includes a copper source and water, and the organic ligand solution includes an organic ligand and ethanol; Furthermore, the Cu-MOF crystals are dispersed in ethanol to form a Cu-MOF crystal solution, which is then mixed with a thioctic acid solution by ultrasound, and then water is added under stirring and the reaction is continued. The material is then washed and vacuum dried to obtain a thioctic acid@Cu-MOF material having dual responses to pH and humidity, wherein the thioctic acid solution includes thioctic acid and ethanol.

[0008] An embodiment of the present invention also provides a thioctic acid@Cu-MOF material having dual responses to pH and humidity obtained by the aforementioned preparation method, wherein thioctic acid in the thioctic acid@Cu-MOF material is loaded on the pores and surface of Cu-MOF through coordination bonds formed between thiol groups (-SH) and copper ions, and the content of thioctic acid in the thioctic acid@Cu-MOF material is 40-60wt%.

[0009] The embodiment of the present invention also provides the use of the aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity in the preparation of fruit and vegetable preservation materials.

[0010] The embodiment of the present invention also provides a composition for preserving fruits and vegetables, which comprises the aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity, sodium alginate, glycerol and water; Among them, the mass volume ratio of sodium alginate to water is 3g:1mL~1g:1mL, the mass volume ratio of glycerol to sodium alginate solution is 1g:100mL~3g:100mL, and the mass ratio of thioctic acid@Cu-MOF material to sodium alginate is 2:1~1:2.

[0011] The embodiment of the present invention also provides a method for preserving fruits and vegetables, which comprises: The aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity, sodium alginate, glycerol and water are uniformly mixed to form a film-forming solution; At least the film-forming solution is coated on the surface of fruits or vegetables, dried, and then stored in an environment with a temperature of 20-30° C. and a humidity of 25-35%.

[0012] Compared with the prior art, the present invention has the following beneficial effects: (1) The preparation method provided by the present invention has low energy consumption, simple operation, low cost and does not require the use of any organic solvent other than anhydrous ethanol during the preparation process; (2) The lipoic acid@Cu-MOF material prepared by the present invention has a high loading capacity and tight coordination; (3) The lipoic acid in the lipoic acid@Cu-MOF material prepared by the present invention can make up for the deficiencies of Cu-MOF in terms of antioxidant and antifungal properties, while Cu-MOF can make up for the deficiencies of lipoic acid in terms of antibacterial properties; (4) The lipoic acid@Cu-MOF material prepared in the present invention controls the release of lipoic acid by responding to changes in pH and humidity in the environment, thereby maximizing the antioxidant and antibacterial effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1a-1hThe SEM images, infrared spectra, potential detection, XRD spectra, nitrogen adsorption curves, specific surface areas and pore size diagrams of the Cu-MOF and thioctic acid@Cu-MOF materials prepared in Comparative Example 1 and Example 1 of the present invention; Figure 2 The colony count diagram of the Cu-MOF and lipoic acid@Cu-MOF materials prepared in Comparative Example 1 and Examples 1, 2, and 3 of the present invention; Figure 3a-3c The antibacterial rates of the Cu-MOF and lipoic acid@Cu-MOF materials prepared in Comparative Example 1 and Examples 1, 2, and 3 of the present invention; Figure 4a-4c The water vapor permeability and antioxidant performance of the thin films made of the membrane solutions prepared in Comparative Example 2 and Example 1 of the present invention and the membrane solutions containing lipoic acid@Cu-MOF materials; Figure 5a-Figure 5b This is a graph showing the pH and humidity response release performance of a thin film made from a membrane solution containing lipoic acid@Cu-MOF material prepared in Example 1 of the present invention; Figure 6a-6f This is a characterization diagram of the application of the membrane solution prepared in Comparative Example 2 and Example 1 of the present invention and the membrane solution containing lipoic acid@Cu-MOF material in the post-harvest preservation of yellow peaches; Figure 7a-7f This is a characterization diagram of the application of the membrane solution prepared in Comparative Example 2 and Example 1 of the present invention and the membrane solution containing lipoic acid@Cu-MOF material in the preservation of post-harvest grapes. DETAILED DESCRIPTION

[0015] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a lipoic acid@Cu-MOF material having dual response to pH and humidity includes: The copper source solution and the organic ligand solution are fully mixed and reacted at 120-150° C. for 12-15 hours, followed by washing and a first drying process, and then the obtained product is immersed in dichloromethane and subjected to vacuum drying to obtain Cu-MOF crystals; wherein the copper source solution includes a copper source and water, and the organic ligand solution includes an organic ligand and ethanol; Furthermore, the Cu-MOF crystals are dispersed in ethanol to form a Cu-MOF crystal solution, which is then mixed with a thioctic acid solution by ultrasound, and then water is added under stirring and the reaction is continued. The material is then washed and vacuum dried to obtain a thioctic acid@Cu-MOF material having dual responses to pH and humidity, wherein the thioctic acid solution includes thioctic acid and ethanol.

[0017] In some preferred embodiments, the copper source includes any one or more combinations of copper nitrate trihydrate, copper chloride, copper sulfate, and copper acetate, but is not limited thereto.

[0018] In some preferred embodiments, the organic ligand includes any one or more combinations of terephthalic acid, phthalic acid, trimesic acid, and 2,5-dihydroxyterephthalic acid, but is not limited thereto.

[0019] In some preferred embodiments, the molar ratio of the copper source to the organic ligand is 1:1 to 3:1; for example, any one of 1:1, 2:1, and 3:1.

[0020] In some preferred embodiments, the temperature of the first drying treatment is 60-100° C. (eg, 80° C.).

[0021] In some preferred embodiments, the soaking time is 12 to 36 hours (eg, 24 hours).

[0022] In some preferred embodiments, the temperature of the vacuum drying treatment is 120-180° C. (eg, 150° C.).

[0023] In some preferred embodiments, the mass ratio of Cu-MOF crystals to lipoic acid in the Cu-MOF crystal solution is 1:1 to 1:5.

[0024] In some preferred embodiments, the mass volume ratio of the Cu-MOF crystals to ethanol is 1 g:100 mL.

[0025] In some preferred embodiments, the mass volume ratio of lipoic acid to ethanol in the lipoic acid solution is 1 g:100 mL.

[0026] In some preferred embodiments, the ultrasonic time is 1 to 3 hours.

[0027] In some preferred embodiments, the stirring time is 1 to 3 hours.

[0028] In some more specific embodiments, the method for preparing the lipoic acid@Cu-MOF material with dual response to pH and humidity comprises the following steps: (1) Dissolve copper nitrate trihydrate in double distilled water and dissolve terephthalic acid in anhydrous ethanol. After fully dissolved, mix the two solutions and stir them thoroughly. Then place the mixture in a polytetrafluoroethylene-lined stainless steel autoclave to react thoroughly at 120°C. After cooling, collect the crystals and wash them. Then, dry them in an oven at 80°C. Then, activate the MOF crystals by soaking them in dichloromethane (during this period, dichloromethane is replaced regularly to completely exchange the water and ethanol attached to the active sites). Then, vacuum dry them at 150°C to obtain Cu-MOF crystals. (2) Take a certain amount of the Cu-MOF crystals in step (1) and add anhydrous ethanol, and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve, then mix the two and ultrasonicate, and then stir the mixed solution. In the initial stage of stirring, slowly add a certain amount of double distilled water to allow thioctic acid to precipitate and be fully wrapped in the Cu-MOF crystals, then wash with anhydrous ethanol, and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material.

[0029] (3) Dissolve a certain amount of sodium alginate in double distilled water and stir evenly, then add a certain amount of glycerol, and then add a certain amount of lipoic acid@Cu-MOF material in step (2), stir evenly and then perform ultrasonic treatment to obtain a membrane solution containing lipoic acid@Cu-MOF material.

[0030] Preferably, after the dissolution in step (1), the two solutions are mixed and stirred thoroughly, and the stirring time is 0.5-1 h.

[0031] Preferably, in step (1), the mixture is placed in a polytetrafluoroethylene-lined stainless steel autoclave for sufficient reaction at 120° C., and the reaction time is 12 h.

[0032] Preferably, after cooling in step (1), the crystals are collected and washed, wherein the washing method is to first wash them by centrifugation with 50% ethanol for 3-5 times, and then wash them by centrifugation with anhydrous ethanol for 3-5 times.

[0033] Preferably, the MOF crystal is activated by soaking in dichloromethane in step (1) (during which the dichloromethane is replaced regularly to completely exchange the water and ethanol attached to the active sites), and the soaking time is 24 hours, with the dichloromethane being replaced every 4-6 hours.

[0034] Preferably, in step (2), a certain amount of the Cu-MOF crystals in step (1) are added to anhydrous ethanol solution, and a certain amount of thioctic acid is added to anhydrous ethanol to be fully dissolved, and then the two are mixed and ultrasonicated, wherein the mass ratio of Cu-MOF crystals to thioctic acid is 1:1, 1:3, 1:5, the mass volume ratio (g / mL) of Cu-MOF to anhydrous ethanol is 1:100, the volume of anhydrous ethanol added to thioctic acid is kept consistent, and the ultrasonication time after mixing is 1-3h.

[0035] Preferably, in step (2), the mixed solution is stirred, and a certain amount of double distilled water is slowly added at the initial stage of stirring to allow lipoic acid to precipitate and fully react with Cu-MOF. The amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system, and the stirring time is 3-5 hours.

[0036] Preferably, in step (3), a certain amount of sodium alginate is dissolved in double distilled water and stirred evenly, and the mass volume ratio (g / mL) of sodium alginate to double distilled water is 3:1, 2:1, or 1:1.

[0037] Preferably, a certain amount of glycerol is added in step (3), and then a certain amount of lipoic acid@Cu-MOF crystals in (2) are added, and the mixture is stirred evenly and then ultrasonically treated. The mass volume ratio of the added amount of glycerol to the total volume of the solution in the system is 1%-3% (g / mL), the mass ratio of lipoic acid@Cu-MOF crystals to sodium alginate is 2:1, 1:1, 1:2, and the ultrasonic time after stirring evenly is 1-3h.

[0038] Another aspect of the embodiment of the present invention further provides a thioctic acid@Cu-MOF material with dual response to pH and humidity obtained by the aforementioned preparation method, wherein thioctic acid in the thioctic acid@Cu-MOF material is loaded on the pores and surface of Cu-MOF through a coordination bond formed by a thiol group (-SH) and a copper ion, and the content of thioctic acid in the thioctic acid@Cu-MOF material is 40~60wt%.

[0039] The lipoic acid@Cu-MOF material in the present invention has dual responses to pH and humidity. The coordination of lipoic acid and Cu-MOF enhances the sensitivity of the material to changes in pH and humidity. Specifically, pH sensitivity: in an acidic environment, the carboxyl group of lipoic acid may be protonated, resulting in the shrinkage of the pores of Cu-MOF and a decrease in adsorption capacity; while in an alkaline environment, the carboxyl group is deprotonated, the pores expand, and the adsorption capacity is enhanced. This dynamic change in the pore structure enables Cu-MOF to adjust its adsorption performance according to the environmental pH value; humidity sensitivity: the introduction of lipoic acid increases the hydrophilicity of the Cu-MOF surface, making it more sensitive to humidity changes. In a high humidity environment, functional groups such as the carboxyl and amino groups of lipoic acid can adsorb more water molecules and fill the pores of Cu-MOF, resulting in a decrease in its specific surface area and porosity, affecting the adsorption and catalytic performance.

[0040] Another aspect of the embodiments of the present invention further provides the use of the aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity in the preparation of fruit and vegetable preservation materials.

[0041] Another aspect of the embodiments of the present invention further provides a composition for preserving fruits and vegetables, which comprises the aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity, sodium alginate, glycerol and water; Among them, the mass volume ratio of sodium alginate to water is 3g:1mL~1g:1mL, the mass volume ratio of glycerol to sodium alginate solution is 1g:100mL~3g:100mL, and the mass ratio of thioctic acid@Cu-MOF material to sodium alginate is 2:1~1:2.

[0042] Another aspect of the embodiments of the present invention further provides a method for preserving fruits and vegetables, comprising: The aforementioned lipoic acid@Cu-MOF material with dual response to pH and humidity, sodium alginate, glycerol and water are uniformly mixed to form a film-forming solution; At least the film-forming solution is coated on the surface of fruits or vegetables, dried, and then stored in an environment with a temperature of 20-30° C. and a humidity of 25-35%.

[0043] In some preferred embodiments, fruits or vegetables are soaked in the aforementioned antibacterial material film-forming solution for fruit and vegetable preservation for 3-7 minutes (e.g., 5 minutes), then taken out and drained, and stored at 25°C and 30% relative humidity, thereby achieving fruit and vegetable preservation. After soaking and draining, a film is formed on the surface of the fruit and vegetable, which has good water and gas barrier properties, good antioxidant and antibacterial properties, is easy to clean, and does not affect the natural breathing of the fruit and vegetable.

[0044] In some preferred embodiments, the mass volume ratio of sodium alginate to water is 3g:1mL~1g:1mL.

[0045] In some preferred embodiments, the mass volume ratio of the glycerol to the sodium alginate solution is 1 g:100 mL to 3 g:100 mL.

[0046] In some preferred embodiments, the mass ratio of the lipoic acid @Cu-MOF material to sodium alginate is 2:1~1:2. The present invention is to first dissolve copper nitrate trihydrate in double distilled water, and dissolve terephthalic acid in anhydrous ethanol. After fully dissolved, the two solutions are mixed and fully stirred, and then the mixture is placed in a polytetrafluoroethylene-lined stainless steel autoclave for full reaction at 120°C. After cooling, the crystals are collected and washed, and then dried in an oven at 80°C. After that, the MOF crystals are activated by soaking in dichloromethane (during this period, the dichloromethane is replaced regularly to completely exchange the water and ethanol attached to the active sites), and then vacuum dried at 150°C to obtain Cu-MOF crystals; a certain amount of Cu-MOF crystals are added to anhydrous ethanol, and a certain amount of lipoic acid is added to anhydrous ethanol to fully dissolve, and then the two are mixed and ultrasonicated. Then the mixed solution is stirred, and a certain amount of double distilled water is slowly added at the initial stage of stirring to precipitate lipoic acid and fully react with Cu-MOF. After that, it was washed with anhydrous ethanol and vacuum dried at 50°C to obtain lipoic acid @Cu-MOF crystals; a certain amount of sodium alginate was dissolved in double distilled water and stirred evenly. Subsequently, a certain amount of glycerol was added, and then a certain amount of lipoic acid @Cu-MOF crystals were added, stirred evenly, and then ultrasonically treated to obtain a membrane solution containing lipoic acid @Cu-MOF material.

[0047] According to the preparation scheme of the present invention, those skilled in the art use conventional experimental methods to optimize and select relevant parameters or technical means such as the type of substance in the reaction, the amount of substance used, the solution concentration, the reaction time, and the separation of the product to obtain the lipoic acid @Cu-MOF material of the present invention.

[0048] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0049] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0050] Example 1 This embodiment provides a method for preparing a lipoic acid@Cu-MOF material with dual response to pH and humidity, which specifically includes the following steps: (1) Copper nitrate trihydrate was dissolved in double distilled water, and terephthalic acid was dissolved in anhydrous ethanol. After being fully dissolved, the two solutions were mixed and stirred for 30 minutes. The mixture was then placed in a polytetrafluoroethylene-lined stainless steel autoclave and reacted at 120°C for 12 hours. After cooling, the crystals were collected and washed three times with 50% ethanol and anhydrous ethanol, respectively, and then dried in an oven at 80°C. The MOF crystals were then activated by soaking in dichloromethane for 24 hours (during this period, the dichloromethane was replaced every 4 hours to completely exchange the water and ethanol attached to the active sites), and then dried in a vacuum at 150°C to obtain Cu-MOF crystals.

[0051] (2) Take a certain amount of the Cu-MOF crystals in step (1) and add anhydrous ethanol (mass volume ratio of 1:100, g / mL), and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve (the mass ratio of Cu-MOF to thioctic acid is 1:3, and the volume of anhydrous ethanol added to thioctic acid is consistent with that in Cu-MOF), then mix the two and ultrasonicate for 2 h, and then stir the mixed solution for 4 h. At the initial stage of stirring, slowly add a certain amount of double distilled water (the amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system) to allow thioctic acid to precipitate and be fully wrapped in Cu-MOF, then wash with anhydrous ethanol, and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material, recorded as: LA@Cu-MOF-0.3.

[0052] (3) Take a certain amount of sodium alginate and dissolve it in double distilled water and stir it evenly (mass volume ratio is 2:1, g / mL), then add 1% (w / v, g / mL) glycerol, and then add a certain amount of thioctic acid@Cu-MOF crystals in (2) (the mass ratio of thioctic acid@Cu-MOF crystals to sodium alginate is 1:1), stir evenly and then ultrasonically treat for 1 hour to obtain a membrane solution containing thioctic acid@Cu-MOF material, then put the harvested fruit into the membrane solution and soak it for 5 minutes, drain it and store it at 25℃ and 30% relative humidity.

[0053] Figure 1a-1h The SEM images, infrared spectra, potential detection, XRD spectra, nitrogen adsorption curves, specific surface areas, and pore size diagrams of the Cu-MOF and thioctic acid@Cu-MOF materials (i.e., LA@Cu-MOF-0.3) prepared in Comparative Example 1 and Example 1, respectively; in the SEM image, it can be seen that the morphology of the thioctic acid@Cu-MOF material has changed, and some substances are attached to the surface, and their size has expanded from the original 4-8 μm to 12-16 μm; in the infrared spectrum, it can be seen that the characteristic peak of the disulfide bond (520cm-1) is lost in the thioctic acid@Cu-MOF material. -1), indicating that after the reaction of lipoic acid with Cu-MOF, the thiol group forms a coordination bond with the copper ion, so that the two can be tightly combined; in the potential image, it can be seen that the potential of the lipoic acid @Cu-MOF material has dropped significantly; in the XRD spectrum, it can be seen that the crystal structures of Cu-MOF and lipoic acid @Cu-MOF materials are very similar, indicating that the reaction of Cu-MOF with lipoic acid does not affect the integrity of its structure; in the nitrogen adsorption curve, specific surface area and pores, it can be seen that Cu-MOF and lipoic acid @Cu-MOF materials have microporous and mesoporous structures; after the reaction of Cu-MOF with lipoic acid, the specific surface area and pores have decreased, which indicates that lipoic acid occupies some of the pores in Cu-MOF after the reaction, thereby reducing the available surface area for gas or other molecules to adsorb. In addition, after the reaction and combination of Cu-MOF with lipoic acid, its encapsulation rate can reach 76.39±0.95%.

[0054] Figure 4a-4c The water vapor permeability and antioxidant activity of the films made from the membrane solutions prepared in Comparative Example 2 and Example 1 and the membrane solutions containing lipoic acid@Cu-MOF material show that the film made from lipoic acid@Cu-MOF material has better water vapor barrier performance and can better prevent water loss; in addition, the film made from lipoic acid@Cu-MOF material has stronger free radical scavenging ability, indicating that its antioxidant performance is stronger.

[0055] Figure 5a-Figure 5b The pH and humidity response release performance of the film made of the membrane solution containing lipoic acid @Cu-MOF material prepared in Example 1 shows that the release amount of lipoic acid in the film made of lipoic acid @Cu-MOF material shows a huge difference under different pH and humidity conditions. As the pH decreases and the humidity increases, lipoic acid will significantly increase its release rate. That is, high humidity conditions and slightly acidic conditions can well promote the release of lipoic acid, indicating that the film made of lipoic acid @Cu-MOF material has good humidity and pH dual response performance.

[0056] Under different humidity conditions, the release rate of lipoic acid in the film varies greatly. As the humidity increases, the release rate of lipoic acid increases. At 30% humidity, the film released a total of 22.16% in a 48-hour period. But at 90% humidity, the film can release 76.50% within 48 hours, far exceeding the release rate under low humidity conditions. Under different pH conditions, the release amount of lipoic acid in the film also has very significant differences. As the pH decreases, the release amount of lipoic acid also increases. At pH 7, the film can only release 101.90mg / L in a 48-hour period. But at pH 5 and 6, the film can release 218.469mg / L and 201.39mg / L within 48 hours, far exceeding the release amount under neutral conditions.

[0057] Figure 6a-6f The membrane solution prepared in Comparative Example 2 and Example 1 and the membrane solution containing lipoic acid@Cu-MOF material (i.e., LA@Cu-MOF-0.3) were used in the post-harvest preservation of yellow peaches. It can be seen that the lipoic acid@Cu-MOF material can significantly reduce the browning degree and weight loss of yellow peaches during storage, inhibit the growth and reproduction of microorganisms, the decrease in hardness and the increase in total soluble solids, thereby effectively inhibiting the rotting and deterioration of yellow peaches.

[0058] Figure 7a-7f The membrane solutions prepared in Comparative Example 2 and Example 1 and the membrane solution containing lipoic acid@Cu-MOF material (i.e., LA@Cu-MOF-0.3) are used in the post-harvest preservation of grapes. It can be seen that the lipoic acid@Cu-MOF material can significantly reduce the browning degree and weight loss of grapes during storage, inhibit the growth and reproduction of microorganisms, the decrease in hardness and the increase in total soluble solids, thereby effectively inhibiting the rotting and deterioration of grapes.

[0059] Comparative Example 1 Copper nitrate trihydrate was dissolved in double distilled water, and terephthalic acid was dissolved in anhydrous ethanol. After fully dissolved, the two solutions were mixed and stirred for 30 minutes, and then the mixture was placed in a polytetrafluoroethylene-lined stainless steel autoclave for reaction at 120°C for 12 hours. After cooling, the crystals were collected and washed with 50% ethanol and anhydrous ethanol three times respectively, and then dried in an oven at 80°C. The MOF crystals were then activated by soaking in dichloromethane for 24 hours (during this period, dichloromethane was replaced every 4 hours to completely exchange the water and ethanol attached to the active sites), and then vacuum dried at 150°C to obtain Cu-MOF crystals.

[0060] Example 2 (1) Dissolve copper nitrate trihydrate in double distilled water and dissolve terephthalic acid in anhydrous ethanol. After fully dissolved, mix the two solutions and stir for 30 minutes. Then place the mixture in a polytetrafluoroethylene-lined stainless steel autoclave and react at 120°C for 12 hours. After cooling, collect the crystals and wash them with 50% ethanol and anhydrous ethanol three times respectively, and then dry them in an oven at 80°C. Then activate the MOF crystals by soaking them in dichloromethane for 24 hours (during this period, dichloromethane was replaced every 4 hours to completely exchange the water and ethanol attached to the active sites), and then vacuum dry them at 150°C to obtain Cu-MOF crystals.

[0061] (2) Take a certain amount of Cu-MOF in step (1) and add anhydrous ethanol (mass volume ratio is 1:100), and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve (the mass ratio of Cu-MOF to thioctic acid is 1:1, and the volume of anhydrous ethanol added to thioctic acid is consistent with that in Cu-MOF), then mix the two and ultrasonicate for 1 hour. Then stir the mixed solution for 3 hours, and slowly add a certain amount of double distilled water (the amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system) at the beginning of stirring to precipitate thioctic acid and fully react with Cu-MOF. Then wash with anhydrous ethanol and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material, recorded as LA@Cu-MOF-0.1.

[0062] (3) Dissolve a certain amount of sodium alginate in double distilled water and stir evenly (mass to volume ratio is 2:1). Then, add 1% (w / v) glycerol and a certain amount of lipoic acid@Cu-MOF crystals in step (2) (the mass ratio of lipoic acid@Cu-MOF crystals to sodium alginate is 1:1), stir evenly and then ultrasonically treat for 1 hour to obtain a membrane solution containing lipoic acid@Cu-MOF material. Then, soak the harvested fruit in the membrane solution for 5 minutes, drain and store at 25°C and 30% relative humidity.

[0063] Figure 2 The colony counts of Cu-MOF and lipoic acid @Cu-MOF materials prepared in Comparative Example 1 and Examples 1, 2, and 3 show that compared with Cu-MOF materials, lipoic acid @Cu-MOF materials can better inhibit the growth of Escherichia coli, Staphylococcus aureus, and Botrytis cinerea, among which lipoic acid @Cu-MOF (1:3) antibacterial material (i.e., LA@Cu-MOF-0.3) has the most significant inhibitory effect. In addition, lipoic acid makes up for the deficiencies of Cu-MOF in antifungal performance, while Cu-MOF makes up for the deficiencies of lipoic acid in antibacterial performance, and the two produce more powerful antibacterial properties after reaction combination.

[0064] Figure 3a-3c The antibacterial rates of Cu-MOF and lipoic acid@Cu-MOF materials prepared in Comparative Example 1 and Examples 1, 2, and 3 show that the lipoic acid@Cu-MOF (1:3) antibacterial material (i.e., LA@Cu-MOF-0.3) prepared in Example 1 has the strongest inhibitory effect on the growth of Escherichia coli, Staphylococcus aureus, and Botrytis cinerea, reaching 92%, 100%, and 93%, respectively.

[0065] Example 3 (1) Copper nitrate trihydrate was dissolved in double distilled water, and terephthalic acid was dissolved in anhydrous ethanol. After being fully dissolved, the two solutions were mixed and stirred for 30 minutes. The mixture was then placed in a polytetrafluoroethylene-lined stainless steel autoclave and reacted at 120°C for 12 hours. After cooling, the crystals were collected and washed three times with 50% ethanol and anhydrous ethanol, respectively, and then dried in an oven at 80°C. The MOF crystals were then activated by soaking in dichloromethane for 24 hours (during this period, the dichloromethane was replaced every 4 hours to completely exchange the water and ethanol attached to the active sites), and then dried in a vacuum at 150°C to obtain Cu-MOF crystals.

[0066] (2) Take a certain amount of Cu-MOF in step (1) and add anhydrous ethanol (mass volume ratio is 1:100, g / mL), and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve (the mass ratio of Cu-MOF to thioctic acid is 1:5, and the volume of anhydrous ethanol added to thioctic acid is consistent with that in Cu-MOF), then mix the two and ultrasonicate for 3 hours. Then stir the mixed solution for 5 hours, and slowly add a certain amount of double distilled water (the amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system) at the beginning of stirring to precipitate thioctic acid and fully react with Cu-MOF. Then wash with anhydrous ethanol and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material, namely LA@Cu-MOF-0.5.

[0067] (3) Take a certain amount of sodium alginate and dissolve it in double distilled water and stir it evenly (mass volume ratio is 2:1, g / mL), then add 1% (w / v, g / mL) glycerol, and then add a certain amount of lipoic acid @Cu-MOF crystals in step (2) (the mass ratio of lipoic acid @Cu-MOF crystals to sodium alginate is 1:1), stir evenly and then ultrasonically treat for 1h to obtain a membrane solution containing lipoic acid @Cu-MOF material. Then, the harvested fruit is placed in the membrane solution and soaked for 5min, drained and stored at 25℃ and 30% relative humidity.

[0068] Example 4 (1) Cupric chloride was dissolved in deionized water, and trimesic acid was dissolved in anhydrous ethanol. After being fully dissolved, the two solutions were mixed and stirred for 30 min. The mixture was then placed in a polytetrafluoroethylene-lined stainless steel autoclave and reacted at 150 °C for 13 h. After cooling, the crystals were collected and washed three times with 50% ethanol and anhydrous ethanol, respectively, and then dried in an oven at 100 °C. The MOF crystals were then activated by soaking in dichloromethane for 24 h (during this period, dichloromethane was replaced every 4 h to completely exchange the water and ethanol attached to the active sites), and then dried in a vacuum oven at 150 °C to obtain Cu-MOF crystals.

[0069] (2) Take a certain amount of Cu-MOF in step (1) and add anhydrous ethanol (mass volume ratio is 1:100, g / mL), and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve (the mass ratio of Cu-MOF to thioctic acid is 1:1, and the volume of anhydrous ethanol added to thioctic acid is consistent with that in Cu-MOF), then mix the two and ultrasonicate for 3 hours. Then stir the mixed solution for 5 hours, and slowly add a certain amount of double distilled water (the amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system) at the beginning of stirring to precipitate thioctic acid and fully react with Cu-MOF. Then wash with anhydrous ethanol and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material.

[0070] (3) Take a certain amount of sodium alginate and dissolve it in double distilled water and stir it evenly (mass volume ratio is 1:1, g / mL), then add 2% (w / v, g / mL) glycerol, and then add a certain amount of lipoic acid @Cu-MOF crystals in step (2) (the mass ratio of lipoic acid @Cu-MOF crystals to sodium alginate is 2:1), stir evenly and then ultrasonically treat for 1 hour to obtain a membrane solution containing lipoic acid @Cu-MOF material. Then, the harvested fruit is placed in the membrane solution and soaked for 3 minutes, drained and stored at 25°C and 30% relative humidity.

[0071] The lipoic acid@Cu-MOF material in this example exhibits excellent freshness-preserving effect, as shown in Table 1 for details.

[0072] Example 5 (1) Copper acetate was dissolved in double distilled water, and 2,5-dihydroxyterephthalic acid was dissolved in anhydrous ethanol. After being fully dissolved, the two solutions were mixed and stirred for 30 minutes. The mixture was then placed in a polytetrafluoroethylene-lined stainless steel autoclave and reacted at 135°C for 15 hours. After cooling, the crystals were collected and washed three times with 50% ethanol and anhydrous ethanol, respectively, and then dried in an oven at 60°C. The MOF crystals were then activated by soaking in dichloromethane for 24 hours (during this period, the dichloromethane was replaced every 4 hours to completely exchange the water and ethanol attached to the active sites), and then dried in a vacuum at 150°C to obtain Cu-MOF crystals.

[0073] (2) Take a certain amount of Cu-MOF in step (1) and add anhydrous ethanol (mass volume ratio is 1:100, g / mL), and take a certain amount of thioctic acid and add anhydrous ethanol to fully dissolve (the mass ratio of Cu-MOF to thioctic acid is 1:3, and the volume of anhydrous ethanol added to thioctic acid is consistent with that in Cu-MOF), then mix the two and ultrasonicate for 3 hours. Then stir the mixed solution for 5 hours, and slowly add a certain amount of double distilled water (the amount of double distilled water added is the same as the total volume of anhydrous ethanol in the system) at the beginning of stirring to precipitate thioctic acid and fully react with Cu-MOF. Then wash with anhydrous ethanol and vacuum dry at 50°C to obtain thioctic acid@Cu-MOF material.

[0074] (3) Take a certain amount of sodium alginate and dissolve it in double distilled water and stir it evenly (mass volume ratio is 3:1, g / mL), then add 3% (w / v, g / mL) glycerol, and then add a certain amount of lipoic acid @Cu-MOF crystals in step (2) (the mass ratio of lipoic acid @Cu-MOF crystals to sodium alginate is 1:2), stir evenly and then ultrasonically treat for 1h to obtain a membrane solution containing lipoic acid @Cu-MOF material. Then, the harvested fruit is placed in the membrane solution and soaked for 7min, drained and stored at 25℃ and 30% relative humidity.

[0075] The lipoic acid@Cu-MOF material in this example exhibits excellent freshness-preserving effect, as shown in Table 1 for details.

[0076] Comparative Example 2 A certain amount of sodium alginate was dissolved in double distilled water and stirred evenly (mass-volume ratio was 2:1). Subsequently, 1% (w / v) glycerol was added, stirred evenly and ultrasonically treated for 1 hour to obtain a membrane solution. The harvested fruit was then placed in the membrane solution and soaked for 5 minutes. After draining, it was stored at 25°C and 30% relative humidity.

[0077] Comparative Example 3 A certain amount of sodium alginate was dissolved in double distilled water and stirred evenly (mass-to-volume ratio was 2:1, g / mL), followed by addition of 1% (w / v, g / mL) of glycerol, and then a certain amount of Cu-MOF crystals in Comparative Example 1 (the mass ratio of Cu-MOF crystals to sodium alginate was 1:1), stirred evenly and subjected to ultrasonic treatment for 1 h to obtain a membrane solution containing Cu-MOF crystals, and then the harvested fruit was immersed in the membrane solution for 5 min, and stored at 25°C and 30% relative humidity after draining.

[0078] Comparative Example 4 A certain amount of sodium alginate was dissolved in double distilled water and stirred evenly (mass-to-volume ratio was 2:1, g / mL), followed by addition of 1% (w / v, g / mL) glycerol and a certain amount of lipoic acid (the mass ratio of lipoic acid to sodium alginate was 1:1), stirred evenly and subjected to ultrasonic treatment for 1 h to obtain a membrane solution containing lipoic acid, and then the harvested fruit was immersed in the membrane solution for 5 min, drained and stored at 25°C and 30% relative humidity.

[0079] Comparative Example 5 A certain amount of sodium alginate was dissolved in double distilled water and stirred evenly (mass-to-volume ratio was 2:1, g / mL), followed by addition of 1% (w / v, g / mL) glycerol, and then a certain amount of lipoic acid and Cu-MOF crystals (the mass ratio of Cu-MOF to lipoic acid was 1:3, and the mass ratio of the sum of Cu-MOF and lipoic acid to sodium alginate was 1:1). After stirring evenly, the mixture was ultrasonically treated for 1 hour to obtain a membrane solution containing lipoic acid. The harvested fruit was then placed in the membrane solution and soaked for 5 minutes. After draining, the mixture was stored at 25°C and 30% relative humidity.

[0080] The membrane solutions prepared in Examples 1-5 and Comparative Examples 2-5 were applied to the post-harvest preservation of yellow peaches. The specific characterization results are shown in Table 1.

[0081] Table 1 ; Among them, DPPH is 1,1-diphenyl-2-trinitrophenylhydrazine, and ABTS is 2,2′-hydrazine-bis-3-ethylbenzothiazoline-6-sulfonic acid.

[0082] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0083] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A method for preparing lipoic acid@Cu-MOF material with dual response to pH and humidity, It is characterized in that include: The copper source solution and the organic ligand solution are fully mixed and reacted at 120-150° C. for 12-15 hours, followed by washing and a first drying process, and then the obtained product is immersed in dichloromethane and subjected to vacuum drying to obtain Cu-MOF crystals; wherein the copper source solution includes a copper source and water, and the organic ligand solution includes an organic ligand and ethanol; Furthermore, the Cu-MOF crystals are dispersed in ethanol to form a Cu-MOF crystal solution, which is then mixed with a thioctic acid solution by ultrasound, and then water is added under stirring and the reaction is continued. The material is then washed and vacuum dried to obtain a thioctic acid@Cu-MOF material having dual responses to pH and humidity, wherein the thioctic acid solution includes thioctic acid and ethanol.

2. The preparation method according to claim 1, Features: The copper source includes any one or more combinations of copper nitrate trihydrate, copper chloride, copper sulfate, and copper acetate; And / or, the organic ligand includes any one or more combinations of terephthalic acid, phthalic acid, trimesic acid, and 2,5-dihydroxyterephthalic acid.

3. The preparation method according to claim 1, Features: The molar ratio of the copper source to the organic ligand is 1:1 to 3:1; And / or, the temperature of the first drying treatment is 60-100°C; And / or, the soaking time is 12 to 36 hours; And / or, the temperature of the vacuum drying treatment is 120-180°C.

4. The preparation method according to claim 1, Features: The mass ratio of the Cu-MOF crystal to lipoic acid is 1:1 to 1:5; And / or, the mass volume ratio of Cu-MOF crystals to ethanol in the Cu-MOF crystal solution is 1 g:100 mL; And / or, the mass volume ratio of thioctic acid to ethanol in the thioctic acid solution is 1 g:100 mL.

5. The preparation method according to claim 1, Features: The ultrasound time is 1 to 3 hours; And / or, the stirring time is 1 to 3 hours.

6. The lipoic acid@Cu-MOF material having dual response to pH and humidity obtained by the preparation method according to any one of claims 1 to 5, Features: The lipoic acid in the lipoic acid@Cu-MOF material is loaded on the pores and surface of Cu-MOF through coordination bonds formed between thiol groups (-SH) and copper ions. The content of lipoic acid in the lipoic acid@Cu-MOF material is 40-60wt%.

7. Use of the lipoic acid@Cu-MOF material with dual response to pH and humidity as claimed in claim 6 in the preparation of fruit and vegetable preservation materials.

8. A composition for preserving fruits and vegetables, It is characterized in that The method comprises the lipoic acid@Cu-MOF material with dual response to pH and humidity as claimed in claim 6, sodium alginate, glycerol and water; Among them, the mass volume ratio of sodium alginate to water is 3g:1mL~1g:1mL, the mass volume ratio of glycerol to sodium alginate solution is 1g:100mL~3g:100mL, and the mass ratio of thioctic acid@Cu-MOF material to sodium alginate is 2:1~1:

2.

9. A method for preserving fruits and vegetables, It is characterized in that include: The lipoic acid@Cu-MOF material with dual response to pH and humidity as claimed in claim 6, sodium alginate, glycerol and water are uniformly mixed to form a film-forming solution; At least the film-forming solution is coated on the surface of fruits or vegetables, dried, and then stored in an environment with a temperature of 20-30° C. and a humidity of 25-35%.

10. The method for preserving fruits and vegetables according to claim 9, Features: The mass volume ratio of the sodium alginate to water is 3g:1mL~1g:1mL, the mass volume ratio of glycerol to the sodium alginate solution is 1g:100mL~3g:100mL, and the mass ratio of thioctic acid@Cu-MOF material to sodium alginate is 2:1~1:2.

Citation Information

Patent Citations

  • Star polymer with terminal containing lipoyl, preparation method thereof, polymer nanoparticles prepared from star polymer, and applications of star polymer

    CN108586722A

  • Cyclodextrin-metal organic framework composition and preparation method thereof

    CN115252814A

  • Preparation method and application of ultrasonic-assisted zein / Cu-MOF carrier membrane for meat freshness monitoring

    CN118258809A

  • Nano material for removing dental plaque and pigment on dental surface as well as preparation method and application of nano material

    CN118615182A

  • Metal organic framework carrier capable of being used for multi-mode tumor treatment as well as preparation method and application of metal organic framework carrier

    CN118767167A

Cited By

  • Biodegradable chitosan-polylipoic acid composite film as well as preparation method and application thereof

    CN120465196A

  • Sulfur coordination Cu monatomic material as well as preparation method and application thereof

    CN120480178A