Pressure-sensitive adhesive for TPU (thermoplastic polyurethane) car cover and preparation method of pressure-sensitive adhesive

By optimizing the composition and proportion of pressure-sensitive adhesives and combining functional monomers, the residual glue and degumming problems during use of TPU car clothes are solved, and the bonding effect is achieved that is high bonding strength and durability is adapted to different environmental conditions.

CN118956300APending Publication Date: 2024-11-15ZHEJIANG LONGYOU DAOMING OPTICAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411192237.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

After use, TPU car coats are prone to residual glue and degumming, and the bonding performance is poor in high-temperature and low-temperature environments, which affects the use effect.

Method used

Using a specific proportion of soft monomers, hard monomers, initiators, solvents and crosslinking additives, optimize the bonding performance and temperature range of pressure-sensitive adhesives, enhance bonding strength and weather resistance through functional monomers, and ensure TPU Good bonding of substrates.

Benefits of technology

It realizes the bonding effect of TPU car clothes without residual glue and high transferability, enhances the bonding strength and durability, avoids degumming, and adapts to different environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015409780000111
    Figure BDA0005015409780000111
  • Figure BDA0005015409780000121
    Figure BDA0005015409780000121
Patent Text Reader

Abstract

The invention discloses a pressure-sensitive adhesive for TPU (thermoplastic polyurethane) car clothing and a preparation method thereof. The pressure-sensitive adhesive comprises a soft monomer, a hard monomer, an initiator, a solvent and a cross-linking aid, and the mass ratio of the soft monomer to the hard monomer to the initiator to the solvent to the cross-linking aid is (20-30): (7-16): (0.05-0.15): (60-65): (0.01-1). The glass transition temperature, molecular weight and distribution and polarity of the pressure-sensitive adhesive are adjusted, and the crosslinking aid is used, so that the temperature resistance and cohesion of the pressure-sensitive adhesive and the binding force of the pressure-sensitive adhesive and a TPU (thermoplastic polyurethane) substrate are remarkably improved, and appearance haze change caused by micro-phase separation is avoided. In the using process, the TPU car cover is good in binding property with a TPU base material and good in car paint adhesiveness, it is guaranteed that the phenomena of degumming and adhesive residue are avoided in the service life of the TPU car cover, and the TPU car cover can be easily removed and is high in mobility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to a pressure-sensitive adhesive for TPU car covers and a preparation method thereof. Background Art

[0002] Car cover is a kind of protective film that is attached to the surface of car paint with polymer materials to protect the original paint and decorate the car body, and can be easily removed at any time. Car cover is mainly made of PVC, TPH and TPU paint protection film. TPU paint protection film has the characteristics of high tension, pulling force, excellent aging resistance and corrosion resistance, which makes it occupy the high-end product market of car paint protection film for a long time and has long-term development potential. However, the surface energy of TPU material is low, and it is difficult to achieve good adhesion using conventional adhesives, which can easily cause the paint protection film to debond, and seriously damage the car paint and affect the use effect. In addition, the paint protection film is an external film, and high temperature and low temperature environments will have a great impact on the service life of the paint protection film adhesive, especially when the temperature difference between day and night outdoors is large, which will cause the molecular chain of the paint protection film adhesive to degrade and produce residual glue.

[0003] At present, the pressure-sensitive adhesive for TPU car covers has the problem of residual glue easily appearing when changing the car cover after long-term use, poor cohesive performance, or degumming, and poor bonding performance with the TPU base film. Therefore, it is necessary to improve the above problems and develop a pressure-sensitive adhesive for TPU car cover that has no residual glue or degumming and is highly transferable. Summary of the invention

[0004] Aiming at the defects of residual adhesive and debonding in the prior art, the present invention provides a new pressure-sensitive adhesive for TPU car cover and a preparation method thereof.

[0005] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:

[0006] A pressure-sensitive adhesive for TPU car cover comprises a soft monomer, a hard monomer, an initiator, a solvent and a cross-linking auxiliary agent, wherein the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent and the cross-linking auxiliary agent is 20-30:7-16:0.05-0.15:60-65:0.01-1.

[0007] Soft monomers provide the required flexibility and viscosity of the pressure-sensitive adhesive, ensuring good adhesion to different surfaces. The adhesive properties and operating temperature range of the pressure-sensitive adhesive can be optimized by adjusting the type and proportion of soft monomers. Hard monomers enhance the cohesion and mechanical strength of the pressure-sensitive adhesive and improve its resistance to wear and chemical corrosion. The hardness and elastic modulus of the pressure-sensitive adhesive can be adjusted by the selection and proportion of hard monomers. Initiators control the start and rate of polymerization to ensure the uniformity and controllability of the reaction. The molecular weight distribution and final properties of the pressure-sensitive adhesive can be affected by the selection of initiators. Solvents adjust the viscosity and fluidity of the pressure-sensitive adhesive for easy coating and processing. They help dissolve and disperse other components to ensure the uniformity of the pressure-sensitive adhesive. Cross-linking aids increase the cross-linking density of the pressure-sensitive adhesive and enhance its temperature resistance, chemical resistance and mechanical strength. The use of cross-linking aids can improve the long-term stability and durability of the pressure-sensitive adhesive.

[0008] By precisely controlling the proportion of each component, the optimal balance of pressure-sensitive adhesive performance is achieved to meet specific application requirements, ensuring the stability and reliability of the pressure-sensitive adhesive under different environmental conditions.

[0009] The present invention significantly improves the temperature resistance, cohesion and binding force of the pressure-sensitive adhesive with the TPU substrate by adjusting the glass transition temperature, molecular weight and distribution, and polarity of the pressure-sensitive adhesive and using a cross-linking auxiliary agent, and does not cause a change in the appearance of haze due to microphase separation. During use, the present invention has good binding properties with the TPU substrate and good adhesion to the car paint, ensuring that the TPU car cover does not have debonding and residual glue during its service life, and can be easily removed with high removability.

[0010] Preferably, the above-mentioned pressure-sensitive adhesive for TPU car cover further includes a functional monomer, and the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent, the cross-linking aid, and the functional monomer is 20-30:7-16:0.05-0.15:60-65:0.01-1:0.01-4.

[0011] The addition of functional monomers can enhance the bonding strength between the pressure-sensitive adhesive and the substrate and provide a more stable bonding effect. Functional monomers can help improve the cohesion of the pressure-sensitive adhesive and reduce debonding during use by participating in the polymerization reaction. Functional monomers have excellent chemical corrosion resistance and can improve the tolerance of the pressure-sensitive adhesive to chemical substances. The addition of functional monomers can improve the performance of the pressure-sensitive adhesive at more temperatures and improve its stability in high or low temperature environments. Functional monomers can improve the hydrolysis resistance of the pressure-sensitive adhesive and extend its service life in humid environments. Functional monomers can increase the flexibility of the pressure-sensitive adhesive, allowing it to better adapt to surfaces of more shapes and sizes. Functional monomers help improve the aging resistance of the pressure-sensitive adhesive and resist erosion by environmental factors such as ultraviolet rays and oxidation. Functional monomers can improve the coating performance of the pressure-sensitive adhesive, making it easier to evenly coat on the substrate. Functional monomers can improve the mechanical strength of the pressure-sensitive adhesive and make it more stable when subjected to mechanical stress. Functional monomers contain reactive functional groups that can promote the cross-linking reaction of the pressure-sensitive adhesive and improve its overall performance. The addition of functional monomers can improve the adaptability of pressure-sensitive adhesives to more environmental conditions, such as weather resistance, pollution resistance, etc. The addition of functional monomers helps to improve the microstructure of pressure-sensitive adhesives, avoid microphase separation, and maintain the consistency of product performance.

[0012] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the soft monomer includes one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, and 2-ethylhexyl acrylate.

[0013] A variety of soft monomers are available to adjust the properties of the pressure-sensitive adhesive, such as viscosity, flexibility and temperature resistance, as needed. Each soft monomer has its own unique bonding properties, and by using them in combination, the bonding properties of the pressure-sensitive adhesive can be optimized to meet more application requirements. The diversity of soft monomers helps to improve the flexibility of the pressure-sensitive adhesive, allowing the car cover to better fit the curves and irregular shapes of the car surface. Different soft monomers have different temperature resistance properties. Through reasonable selection and proportioning, the stability of the pressure-sensitive adhesive in a wide temperature range can be improved. Butyl acrylate and isooctyl acrylate still maintain good flexibility at low temperatures, which helps to improve the application performance of the pressure-sensitive adhesive in low temperature environments. Soft monomers help to improve the tolerance of the pressure-sensitive adhesive to chemicals, thereby protecting the car paint from corrosion. The addition of soft monomers can improve the viscoelasticity of the pressure-sensitive adhesive, so that it has good resilience while maintaining good bonding properties. 2-Ethylhexyl acrylate has good aging resistance, which helps to extend the service life of the pressure-sensitive adhesive. The addition of soft monomers helps to improve the coating performance of the pressure-sensitive adhesive, making it easier to evenly coat on the TPU car cover. By selecting suitable soft monomers, the adaptability of pressure-sensitive adhesives to more environmental conditions can be improved, such as humidity, ultraviolet radiation, etc. The combination of soft monomers and hard monomers helps to improve the cohesion of pressure-sensitive adhesives and reduce debonding during use.

[0014] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the hard monomer is one or more of methyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, acrylamide and styrene.

[0015] The addition of hard monomers improves the hardness and mechanical strength of pressure-sensitive adhesives, making them more resistant to wear and tear. Methyl methacrylate and ethyl methacrylate can improve the resistance of pressure-sensitive adhesives to chemicals. The type and proportion of hard monomers can adjust the glass transition temperature of pressure-sensitive adhesives, thereby affecting their performance at different temperatures. The addition of hard monomers can improve the stability of pressure-sensitive adhesives in high temperature environments and reduce thermal degradation. The combination of hard monomers and soft monomers helps to form a more uniform bonding layer and improve the bonding performance with the substrate. Hard monomers can enhance the cohesion of pressure-sensitive adhesives and reduce internal fractures during stretching or peeling. Acrylamide can improve the water resistance of pressure-sensitive adhesives, allowing them to maintain bonding effects in humid environments. Styrene can improve the stability of pressure-sensitive adhesives to ultraviolet rays and extend the service life when used outdoors. The addition of hard monomers can improve the resistance of pressure-sensitive adhesives to organic solvents and reduce swelling or dissolution caused by solvents. Hard monomers can improve the processing properties of pressure-sensitive adhesives, such as the adaptability of coating, calendering and other processes. Hard monomers help improve the aging resistance of pressure-sensitive adhesives and resist the performance degradation during long-term aging. Hard monomers can enhance the interactions between molecules, such as hydrogen bonds and van der Waals forces, thereby improving the overall performance of pressure-sensitive adhesives. The addition of hard monomers can improve the adaptability of pressure-sensitive adhesives to more environmental conditions, such as weather resistance and pollution resistance. Hard monomers can improve the impact resistance of pressure-sensitive adhesives, allowing them to better maintain integrity when impacted.

[0016] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the initiator includes one or more of an organic peroxide initiator, an azo initiator, and a persulfate initiator.

[0017] These initiators have high initiation efficiency, can quickly start the polymerization reaction, and shorten the reaction induction period. Different types of initiators have different decomposition temperatures and activities. According to the requirements of the polymerization reaction, the appropriate initiator can be selected to achieve precise control of the reaction conditions. These initiators are suitable for a variety of monomers and polymerization systems, providing a wider range of applications. By selecting the right initiator, the molecular weight distribution, molecular structure and physical properties of the polymer can be optimized. These initiators can increase the rate of polymerization and improve production efficiency. Initiators can form thermally stable structures during the polymerization process, thereby improving the thermal stability of the final product. Initiators help maintain the consistency of polymerization in different batches and ensure the repeatability of product quality. Initiators can reduce side reactions during the polymerization process and improve product purity. Initiators can be used in different solvents and environments, which improves the flexibility of formulation design. By controlling the polymerization reaction, the mechanical properties of the polymer, such as tensile strength and toughness, can be improved. The polymers obtained by polymerization using these initiators have better aging resistance and extend the service life of the product. The choice of initiator can affect the solubility and processability of the polymer, facilitating subsequent processing and application. The pressure-sensitive adhesive obtained by polymerization can be used under a wider range of environmental conditions, with improved water resistance, chemical resistance and weather resistance.

[0018] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the initiator includes one or more of dibenzoyl peroxide, dilauroyl peroxide, tert-butyl peroxide-2-ethylhexanoate, tert-amyl peroxide-2-ethylhexanoate, tert-butyl peroxide pivalate, azobisisobutyronitrile, and azobisisoheptylonitrile.

[0019] Initiators have efficient initiation ability, can quickly start polymerization reactions, and improve production efficiency. Different initiators have different reactivity, and appropriate initiators can be selected as needed to control the rate of polymerization reactions. Through the selection and use of initiators, the molecular weight distribution of polymers can be adjusted, affecting the bonding properties and mechanical properties of pressure-sensitive adhesives. The use of efficient initiators can increase the yield of polymerization reactions, reduce the residual unreacted monomers, and improve product purity. The type and amount of initiators can affect the bonding strength, cohesion, and temperature resistance of pressure-sensitive adhesives. Dibenzoyl peroxide and dilauroyl peroxide have good thermal stability, which helps to improve the storage and use safety of pressure-sensitive adhesives. Different initiators are suitable for different reaction conditions, such as temperature, solvent type, etc., which improves the flexibility of formula design. Initiators can improve the aging resistance of pressure-sensitive adhesives and extend their service life. The selection of initiators helps to improve the adaptability of pressure-sensitive adhesives to more environmental conditions, such as weather resistance and chemical resistance. Initiators can affect the processing properties of pressure-sensitive adhesives, such as coating properties and drying speed. Initiators help achieve a more uniform polymerization reaction, reduce local over-polymerization or under-polymerization, and improve product quality. Initiators can adjust the viscoelasticity of pressure-sensitive adhesives to ensure that they maintain good bonding properties under different conditions. Initiators can reduce side reactions during the polymerization process and improve product stability and reliability.

[0020] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the solvent includes one or more of ethyl acetate, butyl acetate, toluene, isopropyl alcohol and acetylacetone.

[0021] Solvents can adjust the viscosity of pressure-sensitive adhesives, making them easier to apply and process. Solvents help dissolve and disperse other components to ensure the uniformity of pressure-sensitive adhesives. The addition of solvents can improve the fluidity of pressure-sensitive adhesives and facilitate their uniform distribution on the substrate. Ethyl acetate and butyl acetate have faster evaporation rates, which help pressure-sensitive adhesives dry quickly. Solvents can improve the storage and use safety of pressure-sensitive adhesives, such as reducing flammability. The choice of solvents can improve the adaptability of pressure-sensitive adhesives to more environmental conditions, such as water resistance and chemical resistance. Solvents can affect the bonding properties of pressure-sensitive adhesives, such as initial adhesion and lasting adhesion. Acetylacetone can be used as a reaction medium to promote the polymerization reaction. Solvents can prevent precipitation or stratification of pressure-sensitive adhesives during storage and use. Solvents can reduce the residue on the substrate after the pressure-sensitive adhesive is dried and improve the bonding quality. The addition of solvents can improve the coating process of pressure-sensitive adhesives and increase production efficiency. Solvents can affect the viscoelasticity of pressure-sensitive adhesives, ensuring that they can maintain good bonding properties under different conditions. A variety of solvent options provide greater flexibility in formulation design, allowing adjustments to be made based on different application requirements of pressure-sensitive adhesives.

[0022] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the cross-linking auxiliary agent includes one or more of German Bayer TDI, German Bayer IPDI, Huntsman ERISYS GA-240, aluminum acetylacetonate, and Mitsubishi Gas TETRAD-C.

[0023] Crosslinking aids can enhance the crosslinking density inside the pressure-sensitive adhesive, thereby improving its cohesion and tear resistance. Crosslinking aids help improve the stability and durability of pressure-sensitive adhesives under extreme temperature conditions. Crosslinking aids can improve the resistance of pressure-sensitive adhesives to chemicals, allowing them to maintain performance in harsh chemical environments. Aluminum acetylacetonate can improve the hydrolysis resistance of pressure-sensitive adhesives and extend their service life in humid environments. Crosslinking aids can improve the mechanical strength of pressure-sensitive adhesives, including tensile strength and elongation at break. Crosslinking aids help improve the aging resistance of pressure-sensitive adhesives and resist erosion by environmental factors such as ultraviolet rays and oxidation. Crosslinking aids can improve the bonding performance between pressure-sensitive adhesives and substrates, providing a more stable bonding effect. Crosslinking aids help form a uniform crosslinking network in the pressure-sensitive adhesive to avoid local over-crosslinking or under-crosslinking. Crosslinking aids can improve the thermal stability of pressure-sensitive adhesives at high temperatures and reduce thermal degradation. Crosslinking aids can improve the processing properties of pressure-sensitive adhesives, such as coating properties and drying speed. Crosslinking aids can adjust the viscoelasticity of pressure-sensitive adhesives to ensure that they maintain good bonding properties under different conditions. The choice of a variety of crosslinking aids increases the flexibility of formula design and can be adjusted according to the different application requirements of pressure-sensitive adhesives. Crosslinking aids can reduce side reactions during the polymerization process and improve product stability and reliability. Crosslinking aids can shorten the curing time of pressure-sensitive adhesives and improve production efficiency.

[0024] Preferably, in the above-mentioned pressure-sensitive adhesive for TPU car cover, the functional monomers include one or more of acrylic acid, β-acryloxypropionic acid, maleic anhydride, acrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

[0025] Acrylic acid and methacrylic acid increase the polarity of the pressure-sensitive adhesive, thereby improving the bonding performance with polar substrates. The addition of functional monomers improves the wettability of the pressure-sensitive adhesive to the substrate, which helps to achieve better bonding. Hydroxyethyl acrylate and hydroxypropyl acrylate provide additional flexibility, allowing the pressure-sensitive adhesive to adapt to the deformation of the substrate. The addition of functional monomers improves the hydrolysis resistance of the pressure-sensitive adhesive, allowing it to maintain stable bonding performance even in humid environments. Maleic anhydride can improve the resistance of the pressure-sensitive adhesive to chemicals and extend its service life. The addition of functional monomers helps to improve the mechanical strength of the pressure-sensitive adhesive, including tensile strength and tear strength. Functional monomers can adjust the viscoelasticity of the pressure-sensitive adhesive to ensure that it maintains good bonding performance under different use conditions. β-Acryloxypropionic acid can improve the thermal stability of the pressure-sensitive adhesive, allowing it to maintain performance even in high temperature environments. Acrylamide can provide additional functions, such as improving the biocompatibility or antibacterial properties of the pressure-sensitive adhesive. Functional monomers contain reactive functional groups that can promote the cross-linking reaction of the pressure-sensitive adhesive and improve its overall performance. The addition of functional monomers improves the adaptability of pressure-sensitive adhesives to different environmental conditions, such as weather resistance and pollution resistance. Functional monomers can improve the processing properties of pressure-sensitive adhesives, such as coating properties and drying speed. Functional monomers help improve the aging resistance of pressure-sensitive adhesives and resist the performance degradation during long-term aging. The selection of multiple functional monomers increases the flexibility of formula design and can be adjusted according to the different application requirements of pressure-sensitive adhesives.

[0026] Preferably, the method for preparing the above-mentioned TPU pressure-sensitive adhesive for car cover comprises the following steps:

[0027] S1: After the soft monomer and the hard monomer are uniformly mixed in a mass ratio of 20-30:7-16, the mixture is divided into two parts, A and B, in a mass ratio of 3:7;

[0028] S2: Add part A to the solvent, pass nitrogen for 28min to 32min, then add the initiator, maintain the reaction temperature at 60℃ to 70℃, and react for 30min to 90min to obtain the reactant C;

[0029] S3: Add the initiator to part B, and then drop it into the reactant C, maintain the temperature at 70℃~80℃, and add it for 1h~3h. After the addition is completed, add the initiator, maintain the temperature at 80℃~90℃, and maintain it for 3h~5h, then cool it to room temperature, add the solvent and stir it evenly to obtain the reactant D;

[0030] S4: Add reactant D to a cross-linking aid and a solvent, stir and mix to obtain a coating solution, apply the solution on the TPU car cover, and then dry the solution to complete the preparation of the pressure-sensitive adhesive for the TPU car cover.

[0031] Step S1 can optimize the mechanical properties and bonding properties of the pressure-sensitive adhesive by precisely controlling the mass ratio of the soft monomer to the hard monomer. Different ratios of the soft monomer to the hard monomer can adjust the flexibility and hardness of the pressure-sensitive adhesive to achieve a balance of performance. By processing parts A and B separately, the timing of adding the initiator and the reaction conditions can be more accurately controlled, thereby controlling the polymerization reaction. Premixing the soft monomer and the hard monomer helps to achieve more uniform polymerization in subsequent reactions.

[0032] Nitrogen protection in step S2 can exclude oxygen, prevent oxidation reaction, and ensure the purity of the polymerization reaction. Nitrogen protection reduces the safety risks of flammable solvents during the reaction process. Nitrogen stirring helps to evenly mix the solvent and part A monomers, creating conditions for the uniform distribution of the initiator. By controlling the reaction temperature at 60°C to 70°C, the rate of the polymerization reaction is adjusted to avoid unevenness caused by too fast polymerization. Under controlled temperature and nitrogen protection, the polymerization reaction can be carried out more evenly, which helps to obtain an ideal molecular weight distribution. Adding an initiator under nitrogen protection can reduce the degradation of the initiator and improve its initiation efficiency. Carrying out a polymerization reaction under controlled conditions can reduce the generation of by-products and improve the purity of the product. Precise control of the polymerization reaction helps to form a uniform polymer network and enhance the cohesion of the pressure-sensitive adhesive.

[0033] Step S3 adds part B to reactant C, which can achieve gradual polymerization and help form a more uniform polymer network. Maintaining the temperature in the range of 70°C to 80°C provides suitable conditions for the polymerization reaction, which helps to improve the reaction efficiency and product quality. The addition time is controlled at 1h to 3h, and the rate of the polymerization reaction can be adjusted as needed to achieve better reaction control. Keeping warm at 80°C to 90°C for 3h to 5h helps the full growth of the molecular chain and improves the molecular weight and performance of the polymer. Extending the insulation time helps to reduce unreacted monomers and initiators and improve the stability and purity of the final product. At the temperature of step S3, it helps to enhance intermolecular interactions, such as hydrogen bonds, van der Waals forces, etc., thereby improving the performance of the pressure-sensitive adhesive. After cooling to room temperature, add the solvent and stir evenly to ensure the uniformity of the reactant D and avoid excessive or low local concentrations.

[0034] Step S4 evenly applies the coating liquid on the TPU car cover to ensure the consistency and coverage of the pressure-sensitive adhesive. Adding a cross-linking aid during the coating process helps to improve the bonding strength between the pressure-sensitive adhesive and the TPU car cover. The addition of a cross-linking aid promotes the cross-linking reaction inside the pressure-sensitive adhesive and enhances its cohesion and stability. The cross-linking reaction improves the temperature resistance of the pressure-sensitive adhesive, allowing it to be used in a wider temperature range. The addition of a cross-linking aid improves the resistance of the pressure-sensitive adhesive to chemicals and extends its service life. The cross-linking effect helps to improve the hydrolysis resistance of the pressure-sensitive adhesive and maintain its performance in a humid environment. The drying step helps to quickly remove the solvent, shorten the production cycle, and improve efficiency. The addition of a cross-linking aid improves the durability of the pressure-sensitive adhesive and maintains its performance during long-term use. The addition of a cross-linking aid helps to adjust the viscoelasticity of the pressure-sensitive adhesive to ensure that it maintains good bonding properties under different conditions.

[0035] Preferably, in the above-mentioned method for preparing a pressure-sensitive adhesive for TPU car cover, in step S1, the mixture also includes a functional monomer, and the mass ratio of the soft monomer, the hard monomer, and the functional monomer is 20-30:7-16:0.01-4.

[0036] The addition of functional monomers can improve the adhesion of pressure-sensitive adhesives to different substrates, providing stronger initial adhesion and holding force. Functional monomers usually provide additional flexibility, allowing the pressure-sensitive adhesive to adapt to the deformation of the substrate without breaking. The addition of functional monomers can adjust the glass transition temperature of the pressure-sensitive adhesive and optimize its performance at a specific temperature. Functional monomers can improve the resistance of pressure-sensitive adhesives to chemicals and are suitable for a wider range of application environments. Functional monomers help improve the mechanical strength of pressure-sensitive adhesives, such as tensile strength and elongation at break. Functional monomers can improve the stability of pressure-sensitive adhesives in humid environments and resist hydrolysis. The addition of functional monomers helps to enhance the cohesion inside the pressure-sensitive adhesive and reduce debonding. Functional monomers can improve the stability of pressure-sensitive adhesives in high temperature environments and extend their service life. Functional monomers can improve the processing properties of pressure-sensitive adhesives, such as coating properties and drying speed. The addition of functional monomers improves the adaptability of pressure-sensitive adhesives to different environmental conditions, such as weather resistance and pollution resistance. The addition of functional monomers helps to reduce side reactions during the polymerization process and improve the stability and reliability of the product. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with specific embodiments, but they are not intended to limit the present invention:

[0038] Example 1

[0039] A pressure-sensitive adhesive for TPU car cover comprises a soft monomer, a hard monomer, an initiator, a solvent and a cross-linking auxiliary agent, wherein the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent and the cross-linking auxiliary agent is 20-30:7-16:0.05-0.15:60-65:0.01-1.

[0040] Preferably, a functional monomer is also included, and the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent, the cross-linking aid and the functional monomer is 20-30:7-16:0.05-0.15:60-65:0.01-1:0.01-4.

[0041] Preferably, the soft monomer includes one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, and 2-ethylhexyl acrylate.

[0042] Preferably, the hard monomer is one or more of methyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, acrylamide and styrene.

[0043] Preferably, the initiator includes one or more of an organic peroxide initiator, an azo initiator, and a persulfate initiator.

[0044] Preferably, the initiator includes one or more of dibenzoyl peroxide, dilauroyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-pivalate, azobisisobutyronitrile, and azobisisoheptylonitrile.

[0045] Preferably, the solvent includes one or more of ethyl acetate, butyl acetate, toluene, isopropanol, and acetylacetone.

[0046] Preferably, the cross-linking aid includes one or more of German Bayer TDI, German Bayer IPDI, Huntsman ERISYS GA-240, aluminum acetylacetonate, and Mitsubishi Gas TETRAD-C.

[0047] Preferably, the functional monomers include one or more of acrylic acid, β-acryloxypropionic acid, maleic anhydride, acrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

[0048] Preferably, a method for preparing a pressure-sensitive adhesive for TPU car cover comprises the following steps:

[0049] S1: After the soft monomer and the hard monomer are uniformly mixed in a mass ratio of 20-30:7-16, the mixture is divided into two parts, A and B, in a mass ratio of 3:7;

[0050] S2: Add part A to the solvent, pass nitrogen for 28min to 32min, then add the initiator, maintain the reaction temperature at 60℃ to 70℃, and react for 30min to 90min to obtain the reactant C;

[0051] S3: Add the initiator to part B, and then drop it into the reactant C, maintain the temperature at 70℃~80℃, and add it for 1h~3h. After the addition is completed, add the initiator, maintain the temperature at 80℃~90℃, and maintain it for 3h~5h, then cool it to room temperature, add the solvent and stir it evenly to obtain the reactant D;

[0052] S4: Add reactant D to a cross-linking aid and a solvent, stir and mix to obtain a coating solution, apply the solution on the TPU car cover, and then dry the solution to complete the preparation of the pressure-sensitive adhesive for the TPU car cover.

[0053] Preferably, in step S1, the mixture further comprises a functional monomer, and the mass ratio of the soft monomer, the hard monomer and the functional monomer is 20-30:7-16:0.01-4.

[0054] The mass ratio of soft monomer, hard monomer, initiator and solvent is 20-30:7-16:0.05-0.15:60-65:0.01-1. The mass ratio of soft monomer, hard monomer, initiator, solvent, crosslinking aid and functional monomer is 20-30:7-16:0.05-0.15:60-65:0.01-1:0.01-4. The soft monomer and hard monomer are uniformly mixed in a mass ratio of 20-30:7-16. The mass ratio of soft monomer, hard monomer and functional monomer is 20-30:7-16:0.01-4.

[0055] In the above case, the mass fraction of the soft monomer can be 20, 25, or 30, the mass fraction of the hard monomer can be 7, 11.5, or 16, the mass fraction of the initiator can be 0.05, 0.1, or 0.15, the mass fraction of the solvent can be 60, 62.5, or 65, the mass fraction of the crosslinking aid can be 0.01, 0.505, or 1, and the mass fraction of the functional monomer can be 0.01, 2.005, or 4.

[0056] In step S2, the nitrogen protection time can be 28 min, 30 min, or 32 min, the reaction temperature can be maintained at 60° C., 65° C., or 70° C., and the reaction time can be 30 min, 60 min, or 90 min.

[0057] In step S3, the temperature can be maintained at 70°C, 75°C, or 80°C, and the dropping time can be 1h, 2h, or 3h. The heat preservation can be maintained at 80°C, 85°C, or 90°C, and the holding time can be 3h, 4h, or 5h.

[0058] Sample 1:

[0059] 22.96 parts of soft monomer, 10.31 parts of hard monomer, 2.53 parts of functional monomer, 64.2 parts of solvent, 0.15 parts of initiator, wherein the soft monomer is butyl acrylate, the hard monomer is methyl acrylate and vinyl acetate, the ratio of methyl acrylate to vinyl acetate is 5:1, the functional monomer is acrylic acid, the solvent is ethyl acetate and toluene, the ratio of ethyl acetate to toluene is 10:1, and the initiator is azobisisobutyronitrile. The ethyl acetate solvent and the toluene solvent are packaged separately and can be added separately in precise parts.

[0060] After the soft monomer, hard monomer and functional monomer are mixed evenly, they are divided into two parts, A and B, at a ratio of 3:7. Part A is added to 27.24 parts of solvent, including 5.84 parts of toluene solvent and 21.40 parts of ethyl acetate solvent, and stirred evenly to obtain reactant C. Reactant C is added to the reactor, heated to 65°C, and nitrogen is passed through for 30 minutes, then 0.038 parts of initiator is added, the reaction temperature is controlled at 65°C, and the reaction is carried out for 1 hour.

[0061] Add 0.019 parts of initiator to part B, stir evenly, and add to the dropping funnel. After the reaction in the reactor in the previous step is completed, heat it to 73°C and add it dropwise to the reactor. Control the temperature at 73°C and add it for 1 hour. Then heat the reactor to 82°C, add 0.06 parts of initiator, and keep it warm for 1 hour. Add the remaining part of the initiator and keep it warm for 3 hours. Cool it to 40°C, add the remaining part of the solvent, stir evenly, and obtain reactant D.

[0062] 100 parts of reactant D, 0.27 parts of German Bayer TDI crosslinking aid, 0.03 parts of Huntsman ERISYS GA-240 crosslinking aid, 25 parts of solvent. Huntsman ERISYS GA-240 crosslinking agent is meta-phenylenediamine tetraglycidylamine, German Bayer TDI crosslinking agent model is L-75, which is toluene diisocyanate, and the solvent is ethyl acetate.

[0063] The reactant D, the cross-linking agent and the solvent were stirred and mixed to obtain a coating solution. The coating solution was coated on a matte release film, baked in an oven at 120°C for 150s, adjusted to a thickness of 25μm, and transferred and compounded to a 50μm PET substrate and a 130μm TPU substrate with a self-healing coating to obtain a PET sample and a car cover sample, respectively.

[0064] Sample 2:

[0065] 100 parts of reactant D of sample 1, 0.15 parts of aluminum acetylacetone crosslinking aid, and 25 parts of solvent. The solvent is ethyl acetate and acetylacetone in a mass ratio of 49:1.

[0066] After the reactant D and the solvent were stirred evenly, a cross-linking agent was added and stirred evenly to obtain a coating solution. The coating solution was coated on a matte release film, baked in an oven at 120°C for 150s, adjusted to a thickness of 25μm, and transferred to a 50μm PET substrate and a 130μm TPU substrate with a self-healing coating to obtain a PET sample and a car cover sample, respectively.

[0067] Imported glue commonly used in the car cover industry was set as a comparative example. Comparative example 1 was Ashland 951059 glue, and comparative example 2 was Henkel 8087 glue. Then sample 1 and sample 2 were taken for testing.

[0068] The steel plate used for the test is the Kejian KJ-6001B peeling force matte test steel plate, and the painted plate is the Geely original car paint plate.

[0069] The peel strength test refers to GB / T 2792-2014 "Test method for peel strength of adhesive tape".

[0070] The initial adhesion test refers to GB / T 31125-2014 "Test method for initial adhesion of adhesive tapes - Ring method".

[0071] The test results are as follows:

[0072] Table 1: PET sample test comparison table

[0073]

[0074] Table 2: Car cover sample test comparison table

[0075]

[0076] The initial peeling force and initial adhesion of Sample 1 and Sample 2 are higher than those of Comparative Example 1 and Comparative Example 2, so that Sample 1-2 will have a better bonding effect during construction and use. The peeling force after aging of Sample 1 and Sample 2 is lower than that of Comparative Example 1 and Comparative Example 2, and in the removability test, Sample 1-2 did not have debonding and residual glue, while Comparative Example 1 and Comparative Example 2 had debonding after 16 days and 12 days respectively, making Sample 1-2 easier to peel off during future replacement and less likely to cause damage to the car paint.

[0077] In conclusion, the above is only a preferred embodiment of the present invention, and all equivalent changes and modifications made within the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A pressure-sensitive adhesive for TPU car cover, characterized in that: The invention comprises a soft monomer, a hard monomer, an initiator, a solvent and a crosslinking aid, wherein the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent and the crosslinking aid is 20-30:7-16:0.05-0.15:60-65:0.01-1.

2. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: It also includes functional monomers, and the mass ratio of the soft monomer, the hard monomer, the initiator, the solvent, the cross-linking aid, and the functional monomer is 20-30:7-16:0.05-0.15:60-65:0.01-1:0.01-4.

3. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The soft monomer includes one or more of ethyl acrylate, butyl acrylate, isooctyl acrylate, lauryl acrylate, and 2-ethylhexyl acrylate.

4. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The hard monomer is one or more of methyl acrylate, methyl methacrylate, ethyl methacrylate, vinyl acetate, acrylamide and styrene.

5. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The initiator includes one or more of an organic peroxide initiator, an azo initiator, and a persulfate initiator.

6. The TPU pressure-sensitive adhesive for car cover according to claim 5, characterized in that: The initiator includes one or more of dibenzoyl peroxide, dilauroyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-amyl peroxy-2-ethylhexanoate, tert-butyl peroxy-pivalate, azobisisobutyronitrile, and azobisisoheptylonitrile.

7. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The solvent includes one or more of ethyl acetate, butyl acetate, toluene, isopropanol, and acetylacetone.

8. The TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The cross-linking aid includes one or more of German Bayer TDI, German Bayer IPDI, Huntsman ERISYS GA-240, aluminum acetylacetonate, and Mitsubishi Gas TETRAD-C.

9. The TPU pressure-sensitive adhesive for car cover according to claim 2, characterized in that: The functional monomers include one or more of acrylic acid, β-acryloxypropionic acid, maleic anhydride, acrylamide, hydroxyethyl acrylate, hydroxypropyl acrylate, methacrylic acid, hydroxyethyl methacrylate, and hydroxypropyl methacrylate.

10. The method for preparing a TPU pressure-sensitive adhesive for car cover according to claim 1, characterized in that: The following steps are involved: S1: After the soft monomer and the hard monomer are uniformly mixed in a mass ratio of 20-30:7-16, the mixture is divided into two parts, A and B, in a mass ratio of 3:7; S2: Add part A to the solvent, pass nitrogen for 28min to 32min, then add the initiator, maintain the reaction temperature at 60℃ to 70℃, and react for 30min to 90min to obtain the reactant C; S3: Add the initiator to part B, and then drop it into the reactant C, maintain the temperature at 70℃~80℃, and add it for 1h~3h. After the addition is completed, add the initiator, maintain the temperature at 80℃~90℃, and maintain it for 3h~5h, then cool it to room temperature, add the solvent and stir it evenly to obtain the reactant D; S4: Add reactant D to a cross-linking aid and a solvent, stir and mix to obtain a coating solution, apply the solution on the TPU car cover, and then dry the solution to complete the preparation of the pressure-sensitive adhesive for the TPU car cover.

11. The method for preparing a TPU pressure-sensitive adhesive for car cover according to claim 10, characterized in that: In step S1, the mixture further includes a functional monomer, and the mass ratio of the soft monomer, the hard monomer, and the functional monomer is 20-30:7-16:0.01-4.

Citation Information

Cited By

  • Acrylic acid pressure-sensitive adhesive for PVC (Polyvinyl Chloride) car cover film and preparation method thereof

    CN121495482A