Degreasing agent for bending-resistant leather and preparation method of degreasing agent

By using microemulsion degreasing agents prepared with composite surfactants and inorganic salts, the problems of poor degreasing effect and environmental pollution of existing leather degreasing agents are solved, and an efficient and stable leather degreasing process is achieved.

CN118957174APending Publication Date: 2024-11-15FENGAN LEATHER
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411263057.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing leather degreasing agents have poor degreasing effect, pollute the environment, and have high production costs. The non-ionic surfactants and acidic lipases used are complex, which affects the degreasing effect and operation difficulty.

Method used

A composite surfactant, cosurfactant, solvent and inorganic salt is used to prepare a microemulsion degreasing agent that resists tortuous leather. A 50-100nm microemulsion is formed by side shock method to adjust the pH value and improve the degreasing effect.

Benefits of technology

It significantly improves the leather degreasing effect and reduces production costs. The degreasing agent is renewable, easy to degrade, has strong stability and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of leather degreasing, provides a degreasing agent for bending-resistant leather and a preparation method of the degreasing agent, and solves the problems that the existing leather degreasing agent is relatively poor in degreasing effect, pollutes the environment and is relatively high in manufacturing cost. Comprising the following raw materials in parts by weight: 30-40 parts of a composite surfactant, 15-25 parts of a cosurfactant, 15-20 parts of a solvent, 20-40 parts of deionized water and 0.5-5 parts of inorganic salt, the composite surfactant is prepared from the following raw materials in parts by weight: 10 to 30 parts of a surfactant A and 10 to 30 parts of a surfactant B.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather degreasing, in particular to a degreasing agent for flexural-resistant leather and a preparation method thereof. Background Art

[0002] Degreasing is one of the key processes in the leather making process. Its main purpose is to remove the oil components in the leather to create conditions for the penetration and combination of chemical materials in the subsequent leather making process. If the leather is not degreased enough, the water repellency of the oil will hinder the penetration and action of the subsequent chemical materials, making the finished leather feel stiff, the surface greasy, the coating fastness poor, and the formation of oil frost and other defects.

[0003] Chinese patent application No. 202310772129.3 discloses a temperature-changing or light-changing process for sheep leather, wherein the process is to sequentially degrease, retannage, neutralize, fill, dye, finish and paint the wet blue leather to obtain the temperature-changing or light-changing sheep leather; the degreasing step is specifically as follows: adding 40-50°C hot water to a drum containing wet blue leather, adding oxalic acid and nonionic surfactant, rotating for 1.3-1.8h, standing for 6-8h, and washing. After washing, the degreasing step also includes secondary degreasing; the secondary degreasing is specifically as follows: adding 40-50°C hot water to a drum containing wet blue leather, adding fatting agent and nonionic surfactant, rotating for 1.3-1.8h, and washing. In the secondary degreasing step, acid lipase is also added to the 40-50°C hot water; the amount of acid lipase added is 0.5-1.5% of the leather mass. This application can improve the temperature-light-changing performance of leather and the durability of the temperature-light-changing performance of sheep leather. However, this process uses non-ionic surfactants and acid lipase as degreasing agents during the degreasing process. The extraction and production process of lipase is relatively complicated, and high purity and high activity need to be guaranteed, which increases the production cost. It also needs to be carried out under specific conditions, such as suitable pH value, temperature, enzyme concentration, etc., which may affect the degreasing effect or cause enzyme inactivation, which increases the difficulty and cost of operation in the production process.

[0004] Chinese patent application No. 202111600967.X discloses a crack-resistant leather fabric and a production method thereof, which includes degreasing, washing, neutralization, washing, retanning and crack resistance, fatliquoring, dyeing, and color fixing. The degreasing is as follows: placing the goat skin in a drum, adding a degreasing agent for pickling, adding 20-30wt% formic acid aqueous solution to adjust the pH of the mixed solution to 2-3, placing the mixed solution in a drum and rotating it for 2-3h, and then discharging the liquid to obtain defatted goat skin, wherein the degreasing agent is a 5-10wt% sodium chloride aqueous solution. The invention obtains a wear-resistant, waterproof and crack-resistant leather fabric by adding a retanning agent and an anti-cracking agent. However, the use of a 5-10wt% sodium chloride aqueous solution as a degreasing agent has a relatively poor degreasing effect, which may lead to the problem of a strong greasy feeling and poor feel on the surface of the finished leather.

[0005] In the degreasing process of leather making, other types of degreasing agents are also used, such as chlorinated alkanes degreasing agents. Although they have strong degreasing ability, they are harmful to the environment and human health. Summary of the invention

[0006] Therefore, in view of the above problems, the present invention provides a degreasing agent for flex-resistant leather and a preparation method thereof, so as to solve the problems that the existing leather degreasing agents have relatively poor degreasing effect, pollute the environment and have high production costs.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] A degreasing agent for flex-resistant leather, comprising the following raw materials in parts by weight: 30-40 parts of a composite surfactant, 15-25 parts of a co-surfactant, 15-20 parts of a solvent, 20-40 parts of deionized water, and 0.5-5 parts of an inorganic salt; the composite surfactant comprises the following raw materials in parts by weight: 10-30 parts of a surfactant A and 10-30 parts of a surfactant B;

[0009] The structural formula of the surfactant A is shown in formula (1):

[0010]

[0011] In the formula, R1 is a straight-chain alkyl group having 10 to 20 carbon atoms, R2 is any one of a hydrogen atom, an amino group, a hydroxyl group and a carboxyl group, and the number of n is 10 to 50;

[0012] The surfactant B is any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium fatty alcohol polyoxyethylene ether carboxylate.

[0013] Furthermore, the particle size of the degreasing agent droplets for the flex-resistant leather is 50-100 nm.

[0014] Furthermore, the degreasing agent for flex-resistant leather has a light blue opalescence.

[0015] Furthermore, the degreasing agent for the flex-resistant leather exhibits a Tyndall effect after being incident with parallel light.

[0016] Furthermore, Sudan III, an oil-soluble dye, and methylene blue, a water-soluble dye, are simultaneously dropped into the degreasing agent for the flex-resistant leather. The diffusion speed of methylene blue in the microemulsion is faster than that of Sudan III.

[0017] Furthermore, the co-surfactant is any one of ethylene glycol, n-propanol, isopropanol and n-butanol.

[0018] Furthermore, the solvent is any one of D-limonene, n-octane, n-pentanol, n-hexanol and n-octanol.

[0019] Furthermore, the inorganic salt is any one of NaCl, Na2SO4, Na2CO3, KCl, K2CO3, K2SO4, CaCl2 and AlCl3·6H2O.

[0020] A method for preparing a degreasing agent for flexural-resistant leather comprises the following steps:

[0021] S1, weighing the surfactant A and the surfactant B according to parts by weight, mixing the two uniformly to obtain the composite surfactant, and setting aside;

[0022] S2, weighing the inorganic salt and deionized water in parts by weight, adding the inorganic salt to the deionized water, raising the temperature to 40-45° C., dissolving and stirring evenly to obtain an aqueous phase mixture;

[0023] S3, adding the co-surfactant and the solvent to the composite surfactant obtained in step S1, mixing them evenly to obtain an oil phase mixture;

[0024] S4. According to the volume ratio of the oil phase mixture to the water phase mixture of 2-3:1, in a vortex mixer, add the water phase mixture dropwise to the oil phase mixture while shaking, continue shaking, and stir until a clear and transparent oil-in-water microemulsion is obtained, add a NaOH solution with a concentration of 20-30% to adjust the pH to 6-7, and obtain the degreasing agent for the flex-resistant leather.

[0025] By adopting the above technical solution, the beneficial effects of the present invention are:

[0026] 1. In surfactant A, R1 is a straight-chain alkyl group with 10-20 carbon atoms, which is a hydrophobic lipophilic group; R2 is any one of a hydrogen atom, an amino group, a hydroxyl group, a carboxyl group, a sodium sulfate group, and a sodium carboxylate group, which is a polar hydrophilic group; the number of n is 10-50. Within a certain range, the larger the n, the more oxygen on the hydrophilic group of the molecule, the more hydrogen bonds can be formed with water, and the better the water solubility; therefore, surfactant A has both hydrophilic and lipophilic properties, so that surfactant A has good solubility in water and organic solvents, and has high stability in the solution system and is not easily affected by strong electrolyte inorganic salts, acids and bases.

[0027] 2. However, the solubility of surfactant A in water will decrease with the increase of temperature within a certain range; surfactant B is an ionic surfactant, so it has a Krafft temperature point, that is, when the temperature rises to a certain point, the solubility will increase rapidly. Therefore, compounding surfactant A and surfactant B to form a composite surfactant can effectively reduce the influence of temperature.

[0028] 3. The composite surfactant contains long-chain alkyl groups. The long-chain surfactant molecules adsorbed and arranged on the interface layer will make the oil-water interface layer very rigid, so that the oil-water interface layer is not easy to bend, resulting in the formation of liquid crystals rather than microemulsions. Therefore, a small molecular weight short-chain alcohol is added as a co-surfactant, which is any one of ethylene glycol, n-propanol, isopropanol and n-butanol. The composite surfactant molecules and short-chain alcohol molecules form mixed adsorption on the oil-water interface layer, and the alcohol molecules will be interspersed between the surfactants to increase the adsorption amount of the surfactant on the interface layer; the addition of short-chain alcohol molecules can also increase the flexibility of the interface layer, making the interface layer easy to bend, increasing the solubilization ability of the oil phase, and making the system easier to form a microemulsion. In addition, the addition of inorganic salts also has a high solubilization ability for the oil phase. Using medium-chain alcohols, which are any one of D-limonene, n-octane, n-pentanol, n-hexanol and n-octanol, as a solvent to prepare a microemulsion degreasing agent has the characteristics of being renewable, easy to degrade and strong in stability.

[0029] 4. The microemulsion leather degreasing agent formed by the preparation method of the present invention not only has the conventional advantages of emulsifier degreasing, but also shows lower surface tension and interfacial tension after being prepared into microemulsion by the composite surfactant, and can wet and penetrate the surface of raw leather faster, deeply emulsify and solubilize grease inside the raw leather fiber, and wrap the grease in the gap between raw leather fibers inside the gel to migrate outside the leather, thereby enhancing the degreasing effect. The droplet size of the microemulsion is 50-100nm, the system is stable, and stratification is not easy to occur. DETAILED DESCRIPTION

[0030] Example 1

[0031] A degreasing agent for flex-resistant leather, comprising the following raw materials in parts by weight: 30 parts of a composite surfactant, 15 parts of n-butanol, 15 parts of D-limonene, 20 parts of deionized water, and 0.5 parts of NaCl; the composite surfactant comprises the following raw materials in parts by weight: 10 parts of surfactant A and 10 parts of surfactant B;

[0032] The structural formula of the surfactant A is shown in formula (2):

[0033]

[0034] The surfactant B is sodium dodecyl sulfate;

[0035] Wherein, the preparation method of the degreasing agent for flexural-resistant leather comprises the following steps:

[0036] S1, weighing the surfactant A and the surfactant B according to parts by weight, mixing the two uniformly to obtain the composite surfactant, and setting aside;

[0037] S2, weighing the NaCl and deionized water in parts by weight, adding the NaCl to the deionized water, raising the temperature to 45° C., dissolving and stirring uniformly to obtain an aqueous phase mixture;

[0038] S3, adding the n-butanol and D-limonene to the composite surfactant obtained in step S1, mixing evenly, to obtain an oil phase mixture;

[0039] S4, according to the volume ratio of the oil phase mixture to the water phase mixture of 2:1, in a vortex mixer, adding the water phase mixture dropwise to the oil phase mixture while shaking, continuing to shake and stir until a clear and transparent oil-in-water microemulsion is obtained, adding a 20% NaOH solution to adjust the pH to 6, and obtaining the degreasing agent for the flex-resistant leather;

[0040] The particle size of the degreasing agent droplets for the flexing-resistant leather is 50nm; the degreasing agent for the flexing-resistant leather has a light blue opalescence; the degreasing agent for the flexing-resistant leather exhibits a Tyndall effect after being incident with parallel light; the oil-soluble dye Sudan III and the water-soluble dye methylene blue are simultaneously dropped into the degreasing agent for the flexing-resistant leather, and the diffusion speed of methylene blue in the microemulsion is faster than that of Sudan III.

[0041] Example 2

[0042] A degreasing agent for flex-resistant leather, comprising the following raw materials in parts by weight: 35 parts of a composite surfactant, 20 parts of ethylene glycol, 18 parts of n-octane, 30 parts of deionized water, and 1 part of CaCl2; the composite surfactant comprises the following raw materials in parts by weight: 20 parts of surfactant A and 20 parts of surfactant B;

[0043] The structural formula of the surfactant A is shown in formula (3):

[0044]

[0045] The surfactant B is sodium dodecyl sulfate;

[0046] Wherein, the preparation method of the degreasing agent for flexural-resistant leather comprises the following steps:

[0047] S1, weighing the surfactant A and the surfactant B according to parts by weight, mixing the two uniformly to obtain the composite surfactant, and setting aside;

[0048] S2, weighing the CaCl2 and deionized water in parts by weight, adding the CaCl2 to the deionized water, raising the temperature to 45° C., dissolving and stirring evenly to obtain an aqueous phase mixture;

[0049] S3, adding the ethylene glycol and n-octane to the composite surfactant obtained in step S1, mixing evenly, to obtain an oil phase mixture;

[0050] S4, according to the volume ratio of the oil phase mixture to the water phase mixture of 2.5:1, in a vortex mixer, add the water phase mixture dropwise to the oil phase mixture while shaking, continue shaking, and stir until a clear and transparent oil-in-water microemulsion is obtained, add a 25% NaOH solution to adjust the pH to 6.5, and obtain the degreasing agent for the flex-resistant leather;

[0051] The particle size of the degreasing agent droplets for the flexing-resistant leather is 60nm; the degreasing agent for the flexing-resistant leather has a light blue opalescence; the degreasing agent for the flexing-resistant leather exhibits a Tyndall effect after being incident with parallel light; the oil-soluble dye Sudan III and the water-soluble dye methylene blue are simultaneously dropped into the degreasing agent for the flexing-resistant leather, and the diffusion rate of methylene blue in the microemulsion is faster than that of Sudan III.

[0052] Example 3

[0053] A degreasing agent for flex-resistant leather, comprising the following raw materials in parts by weight: 40 parts of a composite surfactant, 25 parts of isopropanol, 20 parts of n-pentanol, 40 parts of deionized water, and 3 parts of AlCl3·6H2O; the composite surfactant comprises the following raw materials in parts by weight: 10-30 parts of a surfactant A and 10-30 parts of a surfactant B;

[0054] The structural formula of the surfactant A is shown in formula (4):

[0055]

[0056] The surfactant B is sodium dodecylbenzene sulfonate;

[0057] Wherein, the preparation method of the degreasing agent for flexural-resistant leather comprises the following steps:

[0058] S1, weighing the surfactant A and the surfactant B according to parts by weight, mixing the two uniformly to obtain the composite surfactant, and setting aside;

[0059] S2, weighing the AlCl3·6H2O and deionized water in parts by weight, adding the AlCl3·6H2O to the deionized water, raising the temperature to 45° C., dissolving and stirring uniformly to obtain an aqueous phase mixture;

[0060] S3, adding the isopropanol and n-pentanol to the composite surfactant obtained in step S1, mixing evenly, to obtain an oil phase mixture;

[0061] S4, according to the volume ratio of the oil phase mixture to the water phase mixture of 3:1, in a vortex mixer, adding the water phase mixture dropwise to the oil phase mixture while shaking, continuing to shake and stir until a clear and transparent oil-in-water microemulsion is obtained, adding a 30% NaOH solution to adjust the pH to 7, and obtaining the degreasing agent for the flex-resistant leather;

[0062] The particle size of the degreasing agent droplets for the flexing-resistant leather is 55 nm; the degreasing agent for the flexing-resistant leather has a light blue opalescence; the degreasing agent for the flexing-resistant leather exhibits a Tyndall effect after being incident with parallel light; and the oil-soluble dye Sudan III and the water-soluble dye methylene blue are simultaneously dropped into the degreasing agent for the flexing-resistant leather, and the diffusion rate of methylene blue in the microemulsion is faster than that of Sudan III.

[0063] Example 4

[0064] Select the fatty sheepskin leather for degreasing test, weigh the fatty sheepskin leather sample and record it as m2, put the fatty sheepskin leather in a drum, add 3% of the degreasing agent of the flex-resistant leather prepared in Example 1, Example 2, and Example 3 and 100% water by mass at room temperature, turn on the drum and rotate for 60 minutes, and after the end, gently use filter paper to absorb the free water on the liquid surface, weigh the fatty sheepskin leather sample and cut it into small pieces similar to the size of soybeans, use dichloromethane as solvent, use Soxhlet oil extractor, reflux extraction for 6 hours, the total mass of the extract is recorded as m1, and the mass of the dried sample after extraction is recorded as m3. The degreasing rate a (dry basis) is calculated as shown in formulas (6), (7), and (8):

[0065]

[0066] Where: X - is the percentage of moisture in the sample, %;

[0067] Comparative Example 1

[0068] The difference from Example 4 is that the degreasing agent prepared by the technical solution is not used, but the commercially known Dowellor FG-E degreasing agent is used. The other technical solutions are the same as those of Example 4.

[0069] Table 1 is the degreasing rate test results of the products of Example 4 and Comparative Example 1

[0070] project Example 1 Example 2 Example 3 Comparative Example 1 Degreasing rate (%) 76.34±1.1 76.42±0.5 75.96±0.6 67.1±0.3

[0071] It can be seen from Table 1 that when the usage amount of the degreasing agent is 3%, the microemulsion degreasing agent obtained by the technical solution of the present invention has a higher degreasing rate for the sample fatty scleroderma lucidum than the commercially known degreasing agent, and has a better degreasing effect.

[0072] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.

Claims

1. A degreasing agent for flex-resistant leather, characterized in that: The composite surfactant comprises the following raw materials in parts by weight: 30-40 parts of a composite surfactant, 15-25 parts of a co-surfactant, 15-20 parts of a solvent, 20-40 parts of deionized water, and 0.5-5 parts of an inorganic salt; the composite surfactant comprises the following raw materials in parts by weight: 10-30 parts of a surfactant A and 10-30 parts of a surfactant B; The structural formula of the surfactant A is shown in formula (1): In the formula, R1 is a straight-chain alkyl group having 10 to 20 carbon atoms, R2 is any one of a hydrogen atom, an amino group, a hydroxyl group and a carboxyl group, and the number of n is 10 to 50; The surfactant B is any one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium fatty alcohol polyoxyethylene ether carboxylate.

2. A degreasing agent for flex-resistant leather according to claim 1, characterized in that: The particle size of the degreasing agent emulsion droplets for the flexural-resistant leather is 50-100 nm.

3. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The degreasing agent for flex-resistant leather has a light blue opalescence.

4. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The degreasing agent for flex-resistant leather exhibits a Tyndall effect after being incident with parallel light.

5. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The oil-soluble dye Sudan III and the water-soluble dye methylene blue are simultaneously dropped into the degreasing agent for the flex-resistant leather. The diffusion speed of the methylene blue in the microemulsion is faster than that of Sudan III.

6. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The co-surfactant is any one of ethylene glycol, n-propanol, isopropanol and n-butanol.

7. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The solvent is any one of D-limonene, n-octane, n-pentanol, n-hexanol and n-octanol.

8. The degreasing agent for flex-resistant leather according to claim 1, characterized in that: The inorganic salt is any one of NaCl, Na2SO4, Na2CO3, KCl, K2CO3, K2SO4, CaCl2 and AlCl3·6H2O.

9. A method for preparing a degreasing agent for flexural-resistant leather, characterized in that: The following steps are involved: S1. Weigh the surfactant A and the surfactant B in parts by weight according to claim 1, mix the two uniformly to obtain the composite surfactant, and set aside; S2, weighing the inorganic salt and deionized water in parts by weight, adding the inorganic salt to the deionized water, raising the temperature to 40-45° C., dissolving and stirring evenly to obtain an aqueous phase mixture; S3, adding the co-surfactant and the solvent to the composite surfactant obtained in step S1, mixing them evenly to obtain an oil phase mixture; S4. According to the volume ratio of the oil phase mixture to the water phase mixture of 2-3:1, in a vortex mixer, add the water phase mixture dropwise to the oil phase mixture while shaking, continue shaking, and stir until a clear and transparent oil-in-water microemulsion is obtained, add a NaOH solution with a concentration of 20-30% to adjust the pH to 6-7, and obtain the degreasing agent for the flex-resistant leather.

Citation Information

Patent Citations

  • Freezing-tolerant solubilizing type leather degreasing agent and preparation method thereof

    CN106995862A

  • Mild antibacterial leather degreasing agent as well as preparation method and application thereof

    CN115491443A

  • Microemulsion leather degreasing agent and preparation method thereof

    CN117187448A