Preparation method of uncoated semi-processed electrical steel and iron core
The preparation of uncoated semi-process electrical steel cores through incomplete annealing, secondary cold rolling and blue-blueing processes has solved the problem of poor magnetic properties and punching performance of electrical steels, and achieved high magnetic induction and environmentally friendly motor core production. Meets the development needs of high efficiency, energy saving and low cost motors.
Patent Information
- Application Number
- CN202410955486.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing non-oriented electrical steel has poor magnetic properties and punching performance, and the surface coating contains chromium elements, which is harmful to the human body and the environment, and cannot meet the needs of efficient, energy-saving and low-cost motor development.
Low-carbon and low-silicon cold-rolled electrical steel plates are used to make uncoated semi-process electrical steel motor cores through incomplete annealing, secondary cold rolling, stress-removing annealing and blue-generating processes to control grain size and texture , a dense Fe3O4 oxide film is formed, which replaces the insulating coating, and improves magnetic induction and punching properties.
It realizes a coating-free semi-process electrical steel core with high magnetic induction, environmental protection and high production efficiency, avoids the use of chromium elements, improves the working efficiency and punching efficiency of the motor, and reduces the risk of iron loss and short circuit between laminations.
Smart Images

Figure CN118957393A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical steel, and in particular relates to a method for preparing uncoated semi-process electrical steel and an iron core. Background Art
[0002] As people pay more and more attention to environmental protection and energy saving, more and more motors are needed to be more efficient and energy-saving. Therefore, the development of electrical steel cores with low iron loss and high magnetic induction has become a hot direction for the development of high-efficiency motors.
[0003] Motor core design maximum magnetic induction intensity V2 and maximum magnetic induction intensity B m The motor is in low frequency, if the iron core B m If the value is low, the core torque will decrease and the efficiency will be reduced. Therefore, high B is required at low frequency. m However, many household motors and small motors now actually work at low frequencies, so electrical steel materials are required to have low silicon content and high B m value, thereby improving the working efficiency of the motor.
[0004] Semi-process technology is a production process that fully meets the requirements of high magnetic induction and low iron loss performance of low-carbon and low-silicon electrical steel. However, the semi-process non-oriented electrical steel on the market has poor magnetic properties and punching performance; the iron core is prone to lamination adhesion during annealing, resulting in product scrapping and other problems. It can no longer meet the current development needs of motor high efficiency, energy saving and low manufacturing cost.
[0005] The insulating coating on the surface of non-oriented electrical steel contains chromium. 6+ It is a toxic substance that can be swallowed or inhaled. Skin contact can cause allergies and cancer. It has a lasting harm to the human body and the environment. Therefore, the EU ROHS directive requires that Cr in electronic and electrical products 6+ Content is less than 1000ppm. In addition, the European Union and Japan have completely stopped using chromium-containing coated electrical steel. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing an uncoated semi-process electrical steel and an iron core, which has the advantages of high magnetic induction, high production efficiency and environmental protection.
[0007] The present invention adopts low-carbon and low-silicon electrical steel cold-rolled plates, adopts a semi-process technology route, and has no coating on the surface. By controlling the incomplete annealing process, the secondary cold rolling process, the stress relief annealing process and the bluing process, a coating-free semi-process electrical steel motor core is made.
[0008] To achieve the above object, the present invention provides the following technical solution: a method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition of the low-carbon and low-silicon electrical steel cold-rolled sheet is as follows by weight: C≤0.003%, Si: 0.3%-1.0%, Als: 0.2%-0.3%, Mn: 0.20%-0.50%, O: ≤0.003%, P: 0.01%-0.03%, S≤0.003%, N≤0.003%, and the preparation steps are as follows:
[0009] S1: Degreasing of cold-rolled low-carbon and low-silicon electrical steel sheets;
[0010] S2: The degreased cold-rolled steel sheet is transferred to a continuous furnace for incomplete annealing;
[0011] S3: secondary cold rolling using a cold rolling mill;
[0012] S4: Use high-speed stamping to make uncoated semi-processed electrical steel into motor core stator and rotor punchings;
[0013] S5: performing stress relief annealing;
[0014] S6: Perform bluing process to make uncoated semi-processed electrical steel motor core.
[0015] Preferably, the thickness of the low-carbon and low-silicon electrical steel cold-rolled sheet is 0.5-0.9 mm.
[0016] The specific steps are as follows: before annealing, the cold-rolled steel strip is firstly cleaned with 70-80℃ alkali solution to remove rolling oil and dirt on the surface, so as to prevent the strip from being brought into the furnace to destroy the protective atmosphere components, affect the decarburization efficiency, and even cause carbon increase. After alkali washing, it is brushed with hot water and blown dry;
[0017] During continuous furnace annealing, the furnace tension should be well controlled to ensure good plate shape and magnetic properties, and to reduce transverse iron loss. Under the premise of ensuring good plate shape, the furnace tension should be reduced as much as possible. If the tension is too large, the iron loss will increase significantly, and it is also easy to break the belt. The appropriate process for incomplete annealing of semi-process electrical steel is to set the temperature of the soaking section to 625-750℃×30-180s under a tension of 5.5-10.5MPa in a continuous furnace, annealing to make the recrystallization rate (α) 55%-75%, control the grain size to 20-50μm, and use N2 as the protective atmosphere without H2. Control the cooling rate to exceed 50℃ / s and quickly cool to 300℃ to prevent the precipitation of Fe3C along the grain boundary. Over-aging treatment at 250-300℃×3min can improve the texture and enhance the magnetic properties.
[0018] Preferably, the specific steps are: the steel strip is directly subjected to secondary cold rolling after incomplete annealing, the temperature is controlled to be greater than 150° C., a cold rolling mill is used for secondary cold rolling, the pressing force is 20% to 40%, and the surface of the steel plate is smooth Ra≤15μm;
[0019] When the original grain size after incomplete annealing is 30-60um, after 20%-40% deformation cold rolling, the grain size of the semi-finished product of uncoated semi-process electrical steel is controlled to be 20-30um to ensure the hardness HV is 130-180HV, improve the punching property and dimensional accuracy, promote grain growth during stress relief annealing of the core stator and rotor punching, and significantly reduce the iron loss. m Significantly improved.
[0020] Preferably, the specific steps are: using a high-speed punch press to make uncoated semi-processed electrical steel into motor stator and rotor punchings, improving the hardness and punching properties of the uncoated semi-processed electrical steel, the punching rate can reach 320-400 times / min, and the punching efficiency is improved.
[0021] Preferably, the specific steps are: after degreasing the motor stator and rotor punching sheets, stress relief annealing is performed in a continuous furnace at 750-800°C for 2h under a dry protective atmosphere, such as 85% N2+6.5% CO2+8.5% CO atmosphere.
[0022] Preferably, the specific steps are: bluing treatment is carried out in a furnace at 550°C for 1h to 1.5h, the atmosphere is 43% N2+3% CO2+4% CO+50% H2O water vapor, so that a thin layer of dense Fe3O4 oxide film is formed everywhere on the punching sheet, and the grain diameter after annealing is 200 to 300um.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The dense Fe3O4 oxide film generated by the bluing process can replace the insulating coating on the surface of electrical steel, preventing short circuits between core laminations and increasing eddy current losses, thereby improving electromagnetic performance; the surface of electrical steel is uncoated and does not contain chromium, which is harmless to the human body and the environment and is more in line with environmental protection policies.
[0025] (2) By increasing the P element content, reducing the annealing temperature and the secondary cold rolling process, it is beneficial to improve the material hardness and flatness, thereby improving the punching performance and manufacturing stability. The punching rate can reach 320-400 times / min, improving the core punching efficiency.
[0026] (3) A high pressing rate of 20% to 40% causes deformation of the internal structure, promotes the growth of grain structure during stress relief annealing, and is conducive to strengthening the {100} component and weakening the {111} component, thereby improving the texture and increasing the B m Thereby improving the working efficiency of the motor. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a flow chart of the steps of the present invention;
[0028] Figure 2The microstructure of the finished uncoated semi-processed electrical steel core of Example 1;
[0029] Figure 3 The microstructure of the finished uncoated semi-processed electrical steel core of Example 2;
[0030] Figure 4 The microstructure of the finished uncoated semi-processed electrical steel core of Example 3;
[0031] Figure 5 The microstructure of the finished product of comparative example 1, the uncoated semi-processed electrical steel core;
[0032] Figure 6 The microstructure of the finished product of comparative example 2, the uncoated semi-processed electrical steel core;
[0033] Figure 7 This is the microstructure of the finished product of comparative example 3, the uncoated semi-process electrical steel core. DETAILED DESCRIPTION
[0034] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Implementation Case 1
[0037] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0025%, Si: 0.36%, Als: 0.23%, Mn: 0.35%, O: 0.0029%, P: 0.012%, S: 0.0025%, N: 0.0023%, and the rest is Fe and inevitable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0038] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0039] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 8MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent the precipitation of Fe3C along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0040] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 23%, and the thickness is cold rolled from 0.65mm to 0.5m;
[0041] S4 high-speed stamping: stamping rate can reach 380 times / min;
[0042] S5 stress relief annealing process: After the stator and rotor punchings are degreased, stress relief annealing is performed in a continuous furnace at 750℃×2h in an atmosphere of 85%N2+6.5%CO2+8.5%CO;
[0043] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0044] Implementation Case 2
[0045] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0024%, Si: 0.54%, Als: 0.21%, Mn: 0.33%, O: 0.0029%, P: 0.011%, S: 0.0025%, N: 0.0023%, and the rest is Fe and inevitable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0046] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0047] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 10MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent Fe3C precipitation along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0048] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 28.57%, and the thickness is rolled from 0.7mm to 0.5mm;
[0049] S4 high-speed stamping: stamping rate can reach 400 times / min;
[0050] S5 stress relief annealing process: After the stator and rotor punchings are degreased, they are heated in a continuous furnace with 85% N2 + 6.5% CO2
[0051] Stress relief annealing was performed at 750°C for 2h in +8.5% CO atmosphere;
[0052] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0053] Implementation Case 3
[0054] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0022%, Si: 0.96%, Als: 0.23%, Mn: 0.34%, O: 0.0028%, P: 0.013%, S: 0.0026%, N: 0.0022%, and the rest is Fe and unavoidable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0055] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0056] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 7.5MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent Fe3C precipitation along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0057] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 37.5%, and the thickness is rolled from 0.8mm to 0.5mm;
[0058] S4 high-speed stamping: stamping rate can reach 380 times / min;
[0059] S5 stress relief annealing process: After the stator and rotor punchings are degreased, stress relief annealing is performed in a continuous furnace at 750℃×2h in an atmosphere of 85%N2+6.5%CO2+8.5%CO;
[0060] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0061] Comparative Case 1
[0062] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0022%, Si: 0.96%, Als: 0.23%, Mn: 0.34%, O: 0.0028%, P: 0.013%, S: 0.0026%, N: 0.0022%, and the rest is Fe and unavoidable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0063] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0064] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 6.4MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent the precipitation of Fe3C along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0065] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 15%, and the thickness is rolled from 0.59mm to 0.5mm;
[0066] S4 high-speed stamping: stamping rate up to 320 times / min;
[0067] S5 stress relief annealing process: After the stator and rotor punchings are degreased, they are heated in a continuous furnace with 85% N2 + 6.5% CO2
[0068] Stress relief annealing was performed at 750°C for 2h in +8.5% CO atmosphere;
[0069] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0070] Comparative Case 2
[0071] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0022%, Si: 0.96%, Als: 0.23%, Mn: 0.34%, O: 0.0028%, P: 0.013%, S: 0.0026%, N: 0.0022%, and the rest is Fe and unavoidable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0072] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0073] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 7.3MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent the precipitation of Fe3C along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0074] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 10%, and the thickness is rolled from 0.56-0.55mm to 0.5mm;
[0075] S4 high-speed stamping: stamping rate up to 330 times / min;
[0076] S5 stress relief annealing process: After the stator and rotor punchings are degreased, stress relief annealing is performed in a continuous furnace at 750℃×2h in an atmosphere of 85%N2+6.5%CO2+8.5%CO;
[0077] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0078] Comparative Case 3
[0079] A method for preparing an uncoated semi-process electrical steel and an iron core, wherein the chemical composition is: C: 0.0022%, Si: 0.96%, Als: 0.23%, Mn: 0.34%, O: 0.0028%, P: 0.013%, S: 0.0026%, N: 0.0022%, and the rest is Fe and unavoidable residual elements; the process route is: cold-rolled sheet - degreasing - continuous furnace incomplete annealing - secondary cold rolling - high-speed stamping - stress relief annealing - bluing, and the specific steps include:
[0080] S1 Degreasing: The cold-rolled steel strip is firstly cleaned with 80℃ alkali solution to remove rolling oil and dirt on the surface, then washed with hot water and blown dry;
[0081] S2 continuous furnace incomplete annealing: the soaking section temperature is set to 650℃×120s annealing, the unit tension value is 7.8MPa, the atmosphere is 100% N2, and the cooling rate is controlled to 50℃ / s to quickly cool to 300℃ to prevent Fe3C precipitation along the grain boundary. Over-aging treatment at 300℃×3min can improve the texture and enhance the magnetic properties;
[0082] S3 secondary cold rolling: the steel strip is directly cold rolled after incomplete annealing, the temperature is controlled to be greater than 150°C, the cold rolling mill is used to press down 5%, and the thickness is rolled from 0.53-0.52mm to 0.5mm;
[0083] S4 high-speed stamping: stamping rate can reach 340 times / min;
[0084] S5 stress relief annealing process: After the stator and rotor punchings are degreased, stress relief annealing is performed in a continuous furnace at 750℃×2h in an atmosphere of 85%N2+6.5%CO2+8.5%CO;
[0085] S6 bluing: bluing treatment was carried out at 550℃×1.5h in an atmosphere of 43%N2+3%CO2+4%CO+50%H2O in a furnace.
[0086] The chemical compositions (%) of the embodiments and comparative examples are shown in Table 1.
[0087] Table 1 Chemical composition of each embodiment and comparative example (%)
[0088] Serial number C(%) Si(%) Al(%) Mn(%) O(%) P(%) S(%) N(%) Fe(%) Case 1 0.0025 0.36 0.23 0.35 0.0027 0.012 0.0024 0.0025 the remaining Case 2 0.0024 0.54 0.21 0.33 0.0029 0.011 0.0025 0.0023 the remaining Case 3 0.0022 0.96 0.25 0.34 0.0028 0.013 0.0026 0.0022 the remaining Comparative Example 1 0.0027 0.38 0.24 0.32 0.0025 0.014 0.0025 0.0026 the remaining Comparative Example 2 0.0026 0.35 0.25 0.36 0.0029 0.011 0.0023 0.0027 the remaining Comparative Example 3 0.0028 0.39 0.22 0.39 0.0028 0.012 0.0024 0.0024 the remaining
[0089] The pressing rate and magnetic properties of the finished iron cores of the embodiments and comparative examples are shown in Table 2.
[0090] Table 2: The pressure reduction rate and magnetic properties of the finished cores of the embodiments and comparative examples
[0091] Serial number Pressure rate Punching rate (times / min) Iron loss P1.5 / 50 (W / kg) <![CDATA[Magnetic induction intensity B 50 (T)]]> Average grain size(um) Case 1 23% 380 ≤3.7 ≥1.79 210 Case 2 28.57% 400 ≤3.6 ≥1.80 250 Case 3 37.5% 380 ≤3.2 ≥1.80 270 Comparative Example 1 15% 320 ≤4.5 ≥1.72 165 Comparative Example 2 10 330 ≤4.9 ≥1.72 152 Comparative Example 3 5% 340 ≤5.4 ≥1.73 132
[0092] It can be seen from Table 2 that there are obvious differences in the magnetic properties and stamping performance of the finished iron cores of the embodiment and the comparative example. The embodiment has a higher pressing rate than the comparative example, and the punching performance is better. 1.5 / 50 Lower, magnetic induction B m Higher, and therefore more efficient, motors.
[0093] Combination Figure 2 - Figure 7 It can be seen from the microstructure that for the embodiment, a high pressing rate is more conducive to the growth of grains, which is conducive to strengthening the {100} component and weakening the {111} component, thereby improving the texture and increasing the B m .
[0094] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0095] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing uncoated semi-process electrical steel and iron core, characterized in that: The chemical composition of the steel is as follows by weight: C≤0.003%, Si: 0.3%~1.0%, Als: 0.2%~0.3%, Mn: 0.20%~0.50%, O: ≤0.003%, P: 0.01%~0.03%, S≤0.003%, N≤0.003%. The preparation steps are as follows: S1: Degreasing of cold-rolled low-carbon and low-silicon electrical steel sheets; S2: The degreased cold-rolled steel sheet is transferred to a continuous furnace for incomplete annealing; S3: secondary cold rolling using a cold rolling mill; S4: stamping uncoated semi-processed electrical steel into motor stator and rotor punchings at high speed; S5: performing stress relief annealing on the motor stator and rotor punching sheets; S6: Perform bluing process to make uncoated semi-processed electrical steel motor core.
2. The method for preparing uncoated semi-processed electrical steel according to claim 1, characterized in that: The specific steps of S2 are: during continuous furnace annealing, the tension in the furnace is controlled at 5.5-10.5MPa, the temperature of the soaking section is 625-750℃×30-180s annealing, the recrystallization rate (α) is 55%-75%, the grain size is controlled at 20-50μm, the protective atmosphere is 100% N2, and during the cooling process, the cooling rate is controlled to exceed 40℃ / S to 300℃ to prevent Fe3C from precipitating along the grain boundaries, and aging treatment is performed at 250-300℃×3min.
3. The method for preparing uncoated semi-processed electrical steel according to claim 1, characterized in that: The specific steps of S3 are: the steel strip is directly cold-rolled for the second time after incomplete annealing, the temperature is controlled to be greater than 150°C, and the cold rolling is carried out by a cold rolling mill with a downward pressure of 20% to 40%. The surface of the steel plate is smooth Ra≤15μm; the grain size of the semi-finished uncoated semi-process electrical steel is controlled to be 20 to 30um to ensure the hardness HV is 130 to 180HV.
4. The method for preparing uncoated semi-processed electrical steel according to claim 1, characterized in that: The specific steps of S5 are: after degreasing the motor stator and rotor punching sheets, stress relief annealing is performed in a continuous furnace at 750-800°C for 2h under a dry protective atmosphere, such as 85% N2+6.5% CO2+8.5% CO atmosphere.
5. The method for preparing uncoated semi-processed electrical steel according to claim 1, characterized in that: The specific steps of S6 are: bluing treatment is carried out in a furnace at 550°C for 1h to 1.5h, with an atmosphere of 43% N2+3% CO2+4% CO+50% H2O water vapor, so that a thin layer of dense Fe3O4 oxide film is formed everywhere on the punching sheet, and the grain diameter after annealing is 200 to 300um.
Citation Information
Cited By
Method for preparing Fe-Si-Al magnetic powder core from silicon steel waste
CN121709408A
A method for preparing iron-silicon-aluminum magnetic powder cores using silicon steel waste
CN121709408B