High-temperature-resistant structural wave-absorbing material and preparation method thereof

By alternately aligning the absorbing fiber layer and the absorbing honeycomb layer in the absorbing material, and optimizing the thickness and loss ability of the fiber layer and honeycomb layer, the problems of poor heat dissipation and weak mechanical properties of traditional foam-based materials at medium and high temperatures are solved. It achieves efficient heat dissipation and temperature resistance, and is suitable for high-temperature resistance.

CN119095356APending Publication Date: 2024-12-06BEIJING INST OF ENVIRONMENTAL FEATURES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185836.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional foam-based structured wave absorbing materials have poor heat dissipation, weak mechanical properties and limited temperature resistance under medium and high temperature usage conditions, making it difficult to meet the application needs of high temperature resistance.

Method used

Using a structural absorbing material composed of a skin layer, an absorbing layer and a reflective layer, the absorbing fiber layer and an absorbing honeycomb layer alternately arranged along the thickness direction, and optimized electromagnetic performance by adjusting the thickness and loss capability of the fiber layer and honeycomb layer. , and use porous structure to improve heat dissipation performance.

Benefits of technology

It realizes excellent heat dissipation, mechanical properties and temperature resistance of wave absorbing materials, meets the conditions for medium and high temperature use, and solves the problems of poor heat dissipation and weak mechanical properties of traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095356A_ABST
    Figure CN119095356A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant structural wave-absorbing material and a preparation method thereof, and belongs to the technical field of wave-absorbing materials.The high-temperature-resistant structural wave-absorbing material comprises a skin layer, an absorbing layer and a reflecting layer which are sequentially arranged from outside to inside in the thickness direction, and the absorbing layer comprises wave-absorbing fiber layers and wave-absorbing honeycomb layers which are alternately arranged in the thickness direction; the dielectric loss of the wave-absorbing fiber layer is gradually increased from outside to inside along the thickness direction; the preparation raw material of the wave-absorbing fiber layer is wave-absorbing fiber prepreg; the preparation raw material of the reflecting layer is carbon fiber prepreg; the preparation raw material of the skin layer is a skin prepreg, and the skin prepreg is at least one of a glass fiber prepreg and a quartz fiber prepreg. The structural wave-absorbing material provided by the invention has excellent heat dissipation performance, mechanical property and temperature resistance, can meet the requirements of medium and high temperature resistant use conditions, and solves the problems of poor heat dissipation performance, weak mechanical property, limited temperature resistance and the like of the traditional foam-based wave-absorbing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of absorbing materials, and in particular to a high temperature resistant structural absorbing material and a preparation method thereof. Background Art

[0002] Compared with coated absorbing materials, structural absorbing materials have the advantages of load-bearing capacity, wide absorption bandwidth, and easy maintenance, and have been applied to various types of components for various targets. At present, multi-layer absorbing structures are widely used in components that require integrated absorbing due to their advantages in mechanical and electrical properties. However, the main body of this type of structural absorbing material uses foam material as the impedance matching layer, which has excellent stability and absorbing performance under normal or medium temperature conditions. However, under medium and high temperature conditions, the characteristics of foam such as strong heat storage and slow heat dissipation are not conducive to the application of high-temperature resistant structural absorbing materials.

[0003] Therefore, there is an urgent need to provide a high temperature resistant structural absorbing material. Summary of the invention

[0004] In view of one or more technical problems existing in the prior art, the present invention provides a high-temperature resistant structural absorbing material and a preparation method thereof. The structural absorbing material provided by the present invention has excellent heat dissipation performance, mechanical properties and temperature resistance, can meet the requirements of resistance to medium and high temperature use conditions, and solves the problems of poor heat dissipation, weak mechanical properties, limited temperature resistance, etc. of traditional foam-based absorbing materials.

[0005] In a first aspect, the present invention provides a high temperature resistant structural absorbing material, the high temperature resistant structural absorbing material comprising a skin layer, an absorbing layer and a reflecting layer arranged in sequence from the outside to the inside along the thickness direction:

[0006] The absorbing layer comprises an absorbing fiber layer and an absorbing honeycomb layer alternately arranged along the thickness direction; the dielectric loss of the absorbing fiber layer increases from the outside to the inside along the thickness direction; the raw material for preparing the absorbing fiber layer is absorbing fiber prepreg; the raw material for preparing the reflecting layer is carbon fiber prepreg; the raw material for preparing the skin layer is skin prepreg, and the skin prepreg is at least one of glass fiber prepreg and quartz fiber prepreg.

[0007] Preferably, the raw materials for preparing the wave-absorbing fiber layer include glass fiber cloth and wave-absorbing adhesive film; and / or

[0008] The raw materials for preparing the wave-absorbing honeycomb layer include fiber honeycombs and wave-absorbing adhesive slurry; preferably, the fiber honeycombs are one or more of glass fiber honeycombs and quartz fiber honeycombs.

[0009] Preferably, the thickness of the skin layer is 0.6-0.8 mm; and / or

[0010] The thickness of the reflective layer is 0.6-0.8 mm.

[0011] Preferably, the honeycomb aperture of the wave-absorbing honeycomb layer decreases from the outside to the inside along the thickness direction. Preferably, the honeycomb aperture of the wave-absorbing honeycomb layer is 1 to 4 mm.

[0012] Preferably, the thickness of the absorbing honeycomb layer increases from the outside to the inside along the thickness direction. Preferably, the thickness of the absorbing honeycomb layer is 0.2 mm.

[0013] Preferably, the absorbing adhesive slurry comprises a dielectric absorber, a binder, a solvent, a composite auxiliary agent and a curing agent; preferably, the mass ratio of the dielectric absorber, the binder, the solvent, the composite auxiliary agent and the curing agent is 2-20:80-98:10-35:2-6:0.67-0.82.

[0014] Preferably, the dielectric absorber is one or more of carbon black, graphene, and carbon nanotubes;

[0015] The binder is one of medium-temperature epoxy resin, phenolic resin, and polyimide resin;

[0016] The solvent is ethyl acetate; and / or

[0017] The auxiliary agents include dispersants and leveling agents.

[0018] In a second aspect, the present invention provides a method for preparing the high temperature resistant structural absorbing material according to the first aspect, the preparation method comprising the following steps:

[0019] According to the performance requirements of the absorbing material, the skin prepreg, the absorbing fiber prepreg, the absorbing honeycomb layer and the carbon fiber prepreg are layered and subjected to a first curing molding to obtain a high temperature resistant structural absorbing material.

[0020] Preferably, the preparation method of the absorbing fiber prepreg comprises: laminating glass fiber cloth and absorbing adhesive film, hot melting and calendering to obtain the absorbing fiber prepreg; preferably, the hot melting temperature is 65-75° C. and the pressure is 0.2-0.3 MPa.

[0021] Preferably, the method for preparing the wave-absorbing honeycomb layer comprises: distributing the wave-absorbing adhesive slurry on the surface of the fiber honeycomb, and performing a second curing molding to obtain the wave-absorbing honeycomb; preferably, after curing molding, the fiber honeycomb increases in weight by 5-20%.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] The absorbing layer of the structural absorbing material provided by the present invention comprises an absorbing fiber layer and an absorbing honeycomb layer arranged alternately in the thickness direction. The absorbing fiber layer not only has good mechanical strength and load-bearing capacity, but also can ensure the flatness of the absorbing honeycomb layer; by adjusting the electromagnetic parameters of the absorbing fiber layer and the laying method, the electromagnetic loss performance of the absorbing material can be optimized, the impedance matching and attenuation capacity of the absorbing material can be coordinated, and broadband and efficient microwave attenuation can be achieved.

[0024] Compared with traditional foam-based structural composite materials, the absorbing honeycomb layer in the structural absorbing material provided by the present invention has light weight, high compressive strength, and high rigidity. It is an excellent lightweight and high-strength structural material that can not only bear weight well, but also can be used as an impedance matching layer. By adjusting the thickness and loss capacity of the absorbing honeycomb layer, the electromagnetic performance of the absorbing material can be optimized, and it has stronger operability and design. In addition, since the absorbing honeycomb layer has a porous structure with good heat dissipation performance, by adjusting the types of fibers and resins, the temperature resistance of the material can be regulated to meet the use requirements at different temperatures, and it has good application prospects.

[0025] The structural absorbing material provided by the present invention has excellent heat dissipation performance, mechanical properties and temperature resistance, can meet the requirements of resistance to medium and high temperature use conditions, and solves the problems of poor heat dissipation, weak mechanical properties, limited temperature resistance, etc. of traditional foam-based absorbing materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 1 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided in Example 1 of the present invention;

[0028] Figure 2 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided by Example 2 of the present invention;

[0029] Figure 3 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided by Example 3 of the present invention;

[0030] Figure 4 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided by Example 4 of the present invention;

[0031] Figure 5 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided by Example 5 of the present invention;

[0032] Figure 6 is a graph showing the reflection loss test results of the high temperature resistant structural absorbing material at different frequencies provided by Example 6 of the present invention;

[0033] Figure 7 1 is a graph showing the reflection loss test results of the structural absorbing material provided in Comparative Example 1 of the present invention at different frequencies;

[0034] Figure 8 1 is a graph showing the reflection loss test results of the structural absorbing material provided in Comparative Example 2 of the present invention at different frequencies;

[0035] Fig. 9 This is a graph showing the reflection loss test results of the structural absorbing material provided in Comparative Example 3 of the present invention at different frequencies. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] In a first aspect, the present invention provides a high-temperature resistant structural absorbing material, which comprises a skin layer, an absorbing layer and a reflecting layer which are sequentially arranged from the outside to the inside along the thickness direction: the absorbing layer comprises an absorbing fiber layer and an absorbing honeycomb layer which are alternately arranged along the thickness direction; the dielectric loss of the absorbing fiber layer increases from the outside to the inside along the thickness direction; the raw material for preparing the absorbing fiber layer is absorbing fiber prepreg; the raw material for preparing the reflecting layer is carbon fiber prepreg; the raw material for preparing the skin layer is skin prepreg, and the skin prepreg is at least one of glass fiber prepreg and quartz fiber prepreg.

[0038] The absorbing layer of the structural absorbing material provided by the present invention comprises an absorbing fiber layer and an absorbing honeycomb layer arranged alternately in the thickness direction. The absorbing fiber layer not only has good mechanical strength and load-bearing capacity, but also can ensure the flatness of the absorbing honeycomb layer; by adjusting the electromagnetic parameters of the absorbing fiber layer and the laying method, the electromagnetic loss performance of the absorbing material can be optimized, the impedance matching and attenuation capacity of the absorbing material can be coordinated, and broadband and efficient microwave attenuation can be achieved.

[0039] Compared with traditional foam-based structural composite materials, the absorbing honeycomb layer in the structural absorbing material provided by the present invention has light weight, high compressive strength, and high rigidity. It is an excellent lightweight and high-strength structural material that can not only bear weight well, but also can be used as an impedance matching layer. By adjusting the thickness and loss capacity of the absorbing honeycomb layer, the electromagnetic performance of the absorbing material can be optimized, and it has stronger operability and design. In addition, since the absorbing honeycomb layer has a porous structure with good heat dissipation performance, by adjusting the types of fibers and resins, the temperature resistance of the material can be regulated to meet the use requirements at different temperatures, and it has good application prospects.

[0040] The structural absorbing material provided by the present invention has excellent heat dissipation performance, mechanical properties and temperature resistance, can meet the requirements of medium and high temperature (100-350°C) use conditions, and solves the problems of poor heat dissipation, weak mechanical properties, limited temperature resistance, etc. of traditional foam-based absorbing materials.

[0041] According to some preferred embodiments, the raw materials for preparing the microwave absorbing fiber layer include glass fiber cloth and microwave absorbing adhesive film;

[0042] In some specific embodiments of the present invention, the thickness of the absorbing fiber layer is 0.2 mm, and the thickness of the absorbing adhesive film is 0.1 mm.

[0043] In some preferred embodiments of the present invention, the absorbing film is obtained by casting the absorbing adhesive slurry; the preparation method of the absorbing film includes: coating the absorbing adhesive slurry on centrifugal paper by wet casting method, evaporating the solvent through a drying oven, and obtaining a semi-cured absorbing film.

[0044] According to some preferred embodiments, the raw materials for preparing the wave-absorbing honeycomb layer include fiber honeycombs and wave-absorbing adhesive slurry; preferably, the fiber honeycombs are one or more of glass fiber honeycombs and quartz fiber honeycombs.

[0045] In some specific embodiments of the present invention, the weight gain of the wave-absorbing honeycomb layer increases gradually from the outside to the inside along the thickness direction compared with the fiber honeycomb.

[0046] According to some preferred embodiments, the thickness of the skin layer is 0.6-0.8 mm.

[0047] According to some preferred embodiments, the thickness of the reflective layer is 0.6-0.8 mm.

[0048] According to some preferred embodiments, the honeycomb aperture of the wave-absorbing honeycomb layer decreases from the outside to the inside along the thickness direction. Preferably, the honeycomb aperture of the wave-absorbing honeycomb layer is 1 to 4 mm.

[0049] According to some preferred embodiments, the thickness of the absorbing honeycomb layer increases from the outside to the inside along the thickness direction. Preferably, the thickness of the absorbing honeycomb layer is 1 to 5 mm.

[0050] According to some preferred embodiments, the absorbing adhesive slurry includes a dielectric absorber, a binder, a solvent, a composite auxiliary agent and a curing agent; preferably, the mass ratio of the dielectric absorber, the binder, the solvent, the composite auxiliary agent and the curing agent is 2-20:80-98:10-35:2-6:0.67-0.82.

[0051] According to some preferred embodiments, the dielectric absorber is one or more of carbon black, graphene, and carbon nanotubes.

[0052] According to some preferred embodiments, the binder is one of medium-temperature epoxy resin, phenolic resin, and polyimide resin.

[0053] According to some preferred embodiments, the solvent is ethyl acetate.

[0054] According to some preferred embodiments, the auxiliary agent includes a dispersant and a leveling agent.

[0055] According to some preferred embodiments, the thickness of the structural absorbing material is 8 to 15 mm.

[0056] In a second aspect, the present invention provides a method for preparing the high temperature resistant structural absorbing material according to the first aspect, the preparation method comprising the following steps:

[0057] According to the performance requirements of the absorbing material, the skin prepreg, the absorbing fiber prepreg, the absorbing honeycomb layer and the carbon fiber prepreg are layered and subjected to a first curing molding to obtain a high temperature resistant structural absorbing material.

[0058] According to some preferred embodiments, the preparation method of the absorbing fiber prepreg comprises: after laminating glass fiber cloth and absorbing adhesive film, hot melting and calendering are performed to obtain the absorbing fiber prepreg; preferably, the hot melting temperature is 65-75°C (for example, it can be 65°C, 66°C, 68°C, 70°C, 72°C or 75°C), and the pressure is 0.2-0.3MPa (for example, it can be 0.2MPa, 0.22MPa, 0.24MPa, 0.25MPa, 0.26MPa, 0.28MPa or 0.3MPa). After the absorbing fiber prepreg is obtained, it is packaged in a polyethylene bag and stored in a freezer at -18°C for standby use.

[0059] In some specific embodiments of the present invention, the glass fiber cloth and the absorbing film are laid in a manner as follows: a layer of semi-cured absorbing film is laid on each of the upper and lower sides of the glass fiber cloth.

[0060] The present invention heat-melts the glass fiber cloth and the absorbing adhesive film after laminating to melt the absorbing adhesive film and impregnate it into the glass fiber, and then calenders the obtained absorbing fiber prepreg, which can play a role in bonding the absorbing honeycomb during the curing process after lamination without the need for additional introduction of adhesive film.

[0061] According to some preferred embodiments, the preparation method of the wave-absorbing honeycomb layer comprises: distributing the wave-absorbing adhesive slurry on the surface of the fiber honeycomb, and performing a second curing molding to obtain the wave-absorbing honeycomb; preferably, the fiber honeycomb gains weight by 5 to 20% after curing molding. The weight gain of the fiber honeycomb after curing molding of the present invention is controlled within the above range to ensure that the wave-absorbing honeycomb layer has excellent electromagnetic loss performance. If the weight gain is too large, the coating on the surface of the fiber honeycomb is easy to fall off.

[0062] In some specific embodiments of the present invention, the fiber honeycomb is at least one of a glass fiber honeycomb and a quartz fiber honeycomb; and the curing molding is performed by vacuum bag molding or autoclave molding.

[0063] The present invention does not specifically limit the temperature of the first curing molding and the second curing molding, and is adjusted according to the type of the binder. For example, the curing temperature of the medium-temperature epoxy resin is 120-135°C, the curing temperature of the phenolic resin is 170-180°C, and the curing temperature of the polyimide resin is 365-375°C; the heating rate is 2-3°C / min, and the holding time is 1-3h.

[0064] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the examples. The present invention does not specifically limit the sources of the reagents used in the examples and comparative examples, and they can be directly purchased or synthesized by themselves. Figure 1-9 The unit of the horizontal axis frequency is GHz, and the unit of the vertical axis reflectivity is dB.

[0065] Example 1

[0066] Preparation of microwave absorbing adhesive slurry:

[0067] 83.2g of carbon black, 2000g of medium-temperature epoxy resin, 208g of ethyl acetate, 125g of composite additive (75g of KH560 dispersant and 50g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 1# absorbing adhesive slurry;

[0068] 173.6g of carbon black, 2000g of medium-temperature epoxy resin, 370g of ethyl acetate, 130g of composite additive (78g of KH560 dispersant and 52g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 2# absorbing adhesive slurry;

[0069] 272.4g of carbon black, 2000g of medium-temperature epoxy resin, 523g of ethyl acetate, 136g of composite additive (82g of KH560 dispersant and 54g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 3# absorbing adhesive slurry;

[0070] 380.9g of carbon black, 2000g of medium-temperature epoxy resin, 690g of ethyl acetate, 143g of composite additive (86g of KH560 dispersant and 57g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 4# absorbing adhesive slurry;

[0071] 500g of carbon black, 2000g of medium-temperature epoxy resin, 875g of ethyl acetate, 150g of composite additive (90g of KH560 dispersant and 60g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 5# absorbing adhesive slurry;

[0072] Preparation of absorbing film:

[0073] The 2#~5# absorbing adhesive slurry was coated on the centrifugal paper by wet casting method with a thickness of 0.1mm. After drying in a 40℃ oven for 30min, the 2#~5# semi-cured absorbing adhesive film was obtained.

[0074] Preparation of absorbing glass fiber prepreg: After laying a piece of the same semi-cured absorbing adhesive film on the upper and lower sides of the glass fiber cloth (using absorbing adhesive films 2# to 5# for the same laying), hot melting is carried out at 70°C and 0.2MPa pressure to melt the absorbing adhesive film and impregnate the glass fiber cloth, and then calendering is carried out to obtain 2# to 5# absorbing glass fiber prepreg with a thickness of 0.2mm; 2# to 5# absorbing glass fiber prepreg is packaged in a polyethylene bag and stored in a freezer at -18°C.

[0075] Preparation of microwave-absorbing honeycombs: Spray 1# microwave-absorbing adhesive slurry on 1# glass fiber honeycomb (thickness is 2mm, the aperture of honeycomb hole is 1.83mm) and 2# glass fiber honeycomb (thickness is 3mm, the aperture of honeycomb hole is 2.75mm), spray 2# microwave-absorbing adhesive slurry on 3# glass fiber honeycomb (thickness is 4mm, the aperture of honeycomb hole is 3.67mm), then heat up to 135℃ at 2℃ / min and keep warm for 2h to solidify and form, and obtain 1# to 3# microwave-absorbing honeycombs with weight gain of 5%, 8% and 10% respectively.

[0076] Laying: Laying layers on the mold in the following order from bottom to top: release cloth, reflective layer (carbon fiber prepreg) with a thickness of 0.4mm, 5# absorbing glass fiber prepreg with a thickness of 0.2mm, 3# absorbing honeycomb, 4# absorbing glass fiber prepreg with a thickness of 0.2mm, 2# absorbing honeycomb, 3# absorbing glass fiber prepreg with a thickness of 0.2mm, 1# absorbing honeycomb, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, 0.6mm thick skin (glass fiber prepreg), and release cloth.

[0077] Curing and molding: After the laying is completed, it is placed in a vacuum bag for evacuation (pressure is 0.1MPa), and placed in an autoclave for curing (pressure is 0.3MPa). The temperature is raised to 135℃ at a heating rate of 2℃ / min for curing. After keeping warm for 2h, the temperature is lowered with the furnace. After it drops to room temperature, the vacuum pressure is released to obtain a high-temperature resistant structural absorbing material.

[0078] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was performed according to GJB2038A-2011. The results are as follows: Figure 1 As shown, it can be seen that the absorbing material prepared in this embodiment has excellent reflection loss performance in the range of 2 to 18 GHz, and the reflection loss is substantially less than -10 dB.

[0079] Example 2

[0080] Preparation of microwave absorbing adhesive slurry:

[0081] 40.8g of carbon black, 2000g of phenolic resin, 204g of ethyl acetate, 122g of composite additive (73g of KH560 dispersant and 49g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min, and after stirring, they were ground three times using an S150 three-roll grinder to obtain 1# absorbing adhesive slurry;

[0082] 127.6g of carbon black, 2000g of phenolic resin, 298g of ethyl acetate, 128g of composite additive (77g of KH560 dispersant and 51g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 2# absorbing adhesive slurry;

[0083] 222.2g of carbon black, 2000g of phenolic resin, 444g of ethyl acetate, 133g of composite additive (80g of KH560 dispersant and 53g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 3# absorbing adhesive slurry;

[0084] 325.6g of carbon black, 2000g of phenolic resin, 605g of ethyl acetate, 140g of composite additive (84g of KH560 dispersant and 56g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 4# absorbing adhesive slurry;

[0085] 439g of carbon black, 2000g of phenolic resin, 780g of ethyl acetate, 146g of composite additives (88g of KH560 dispersant and 58g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, a S150 three-roll grinder was used to grind three times to obtain 5# absorbing adhesive slurry.

[0086] Preparation of microwave-absorbing adhesive film: 2# to 5# semi-cured microwave-absorbing adhesive films were prepared in the same manner as in Example 1.

[0087] Preparation of microwave absorbing glass fiber prepreg: 2# to 5# microwave absorbing glass fiber prepregs were prepared in the same manner as in Example 1.

[0088] Preparation of microwave-absorbing honeycombs: After spraying 1# microwave-absorbing adhesive slurry on 1# glass fiber honeycomb (thickness of 3mm, honeycomb hole diameter of 1.83mm), 2# glass fiber honeycomb (thickness of 4mm, honeycomb hole diameter of 2.75mm) and 3# glass fiber honeycomb (thickness of 5mm, honeycomb hole diameter of 3.67mm), the temperature was raised to 180°C at 2°C / min and kept warm for 2h to solidify and form 1# to 3# microwave-absorbing honeycombs with weight gains of 5%, 10% and 20% respectively.

[0089] Laying: The laying order is the same as in Example 1.

[0090] Curing and molding: After the laying is completed, it is placed in a vacuum bag for evacuation (pressure is 0.1MPa), and placed in an autoclave for curing (pressure is 0.3MPa). The temperature is raised to 180℃ at a heating rate of 2℃ / min for curing. After keeping warm for 2h, the temperature is lowered with the furnace. After it drops to room temperature, the vacuum pressure is released to obtain a high-temperature resistant structural absorbing material.

[0091] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 2 As shown, the absorbing material prepared in this embodiment has good reflection loss performance in the range of 2 to 18 GHz, and the reflection loss in the C to Ku band (4 to 18 GHz) is substantially less than -10 dB.

[0092] Example 3

[0093] Preparation of microwave absorbing adhesive slurry:

[0094] 83.2g of carbon black, 2000g of polyimide resin, 208g of ethyl acetate, 125g of composite auxiliary agent (75g of KH560 dispersant and 50g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min, and after stirring, they were ground three times using an S150 three-roll grinder to obtain 1# absorbing adhesive slurry;

[0095] 127.6g of carbon black, 2000g of polyimide resin, 298g of ethyl acetate, 128g of composite auxiliary agent (77g of KH560 dispersant and 51g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min, and after stirring, they were ground three times using an S150 three-roll grinder to obtain 2# absorbing adhesive slurry;

[0096] 272.4 g of carbon black, 2000 g of polyimide resin, 523 g of ethyl acetate, 136 g of composite auxiliary agent (82 g of KH560 dispersant and 54 g of Digo leveling agent) and 16.7 g of curing agent were stirred and mixed at a speed of 1000 r / min for 30 min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 3# absorbing adhesive slurry;

[0097] 325.6g of carbon black, 2000g of polyimide resin, 605g of ethyl acetate, 140g of composite auxiliary agent (84g of KH560 dispersant and 56g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 4# absorbing adhesive slurry;

[0098] 500g of carbon black, 2000g of polyimide resin, 875g of ethyl acetate, 150g of composite additive (90g of KH560 dispersant and 60g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, a S150 three-roll grinder was used to grind three times to obtain 5# absorbing adhesive slurry.

[0099] Preparation of microwave absorbing adhesive film: Prepare 2# to 5# semi-cured microwave absorbing adhesive films by the same method as in Example 1;

[0100] Preparation of microwave absorbing glass fiber prepreg: 2# to 5# microwave absorbing glass fiber prepregs were prepared in the same manner as in Example 1.

[0101] Preparation of microwave-absorbing honeycombs: Spray 1# microwave-absorbing adhesive slurry on 1# glass fiber honeycomb (thickness is 3mm, the aperture of honeycomb hole is 1.83mm) and 2# glass fiber honeycomb (thickness is 3mm, the aperture of honeycomb hole is 2.75mm), spray 2# microwave-absorbing adhesive slurry on 3# glass fiber honeycomb (thickness is 3mm, the aperture of honeycomb hole is 3.67mm), then heat up to 370℃ at 2℃ / min and keep warm for 2h to solidify and form, and obtain 1# to 3# microwave-absorbing honeycombs with weight gains of 5%, 8% and 12%, respectively.

[0102] Laying: The laying order is the same as in Example 1.

[0103] Curing and molding: After the laying is completed, it is placed in a vacuum bag for evacuation (pressure is 0.1MPa), and placed in an autoclave for curing (pressure is 0.3MPa). The temperature is raised to 370℃ at a heating rate of 2℃ / min for curing. After keeping warm for 2h, the temperature is lowered with the furnace. After it drops to room temperature, the vacuum pressure is released to obtain a high-temperature resistant structural absorbing material.

[0104] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 3 As shown, the reflection loss of the absorbing material prepared in this embodiment is substantially less than -10 dB in the C to Ku band (4 to 18 GHz).

[0105] Example 4

[0106] Preparation of microwave absorbing adhesive slurry:

[0107] 40.8g of carbon black, 2000g of medium-temperature epoxy resin, 204g of ethyl acetate, 122g of composite additive (73g of KH560 dispersant and 49g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 1# absorbing adhesive slurry;

[0108] 173.6g of carbon black, 2000g of medium-temperature epoxy resin, 370g of ethyl acetate, 130g of composite additive (78g of KH560 dispersant and 52g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 2# absorbing adhesive slurry;

[0109] 272.4g of carbon black, 2000g of medium-temperature epoxy resin, 523g of ethyl acetate, 136g of composite additive (82g of KH560 dispersant and 54g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 3# absorbing adhesive slurry;

[0110] 325.6g of carbon black, 2000g of medium-temperature epoxy resin, 605g of ethyl acetate, 140g of composite additive (84g of KH560 dispersant and 56g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, an S150 three-roll grinder was used to grind three times to obtain 4# absorbing adhesive slurry;

[0111] 439g of carbon black, 2000g of medium-temperature epoxy resin, 780g of ethyl acetate, 146g of composite additives (88g of KH560 dispersant and 58g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, a S150 three-roll grinder was used to grind three times to obtain 5# absorbing adhesive slurry.

[0112] Preparation of microwave-absorbing adhesive film: 2# to 5# semi-cured microwave-absorbing adhesive films were prepared in the same manner as in Example 1.

[0113] Preparation of microwave absorbing glass fiber prepreg: 2# to 5# microwave absorbing glass fiber prepregs were prepared in the same manner as in Example 1.

[0114] Preparation of microwave-absorbing honeycomb: 1# After spraying the microwave-absorbing adhesive slurry on 1# glass fiber honeycomb (thickness is 2mm, the aperture of the honeycomb hole is 2.75mm), the temperature is raised to 135°C at 2°C / min and kept for 2h to solidify and form, and 1# microwave-absorbing honeycomb is obtained, and the weight gain is 10%.

[0115] Laying: Laying layers on the mold in the following order from bottom to top: release cloth, 0.4mm thick reflective layer (carbon fiber prepreg), 0.2mm thick 5# absorbing glass fiber prepreg, 1# absorbing honeycomb, 0.2mm thick 4# absorbing glass fiber prepreg, 1# absorbing honeycomb, 0.2mm thick 3# absorbing glass fiber prepreg, 1# absorbing honeycomb, 0.2mm thick 2# absorbing glass fiber prepreg, 0.6mm skin (glass fiber prepreg), and release cloth.

[0116] Curing and molding: After the laying is completed, it is placed in a vacuum bag for evacuation (pressure is 0.1MPa), and placed in an autoclave for curing (pressure is 0.3MPa). The temperature is raised to 135℃ at a heating rate of 2℃ / min for curing. After keeping warm for 2h, the temperature is lowered with the furnace. After it drops to room temperature, the vacuum pressure is released to obtain a high-temperature resistant structural absorbing material.

[0117] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 4 As shown, the reflection loss of the absorbing material prepared in this embodiment is substantially less than -10 dB in the C to Ku band (4-18 GHz).

[0118] Example 5

[0119] It is basically the same as Example 1, with the only differences being: 1# glass fiber honeycomb (thickness is 2 mm, the aperture of the honeycomb hole is 2.75 mm), 2# glass fiber honeycomb (thickness is 3 mm, the aperture of the honeycomb hole is 2.75 mm), and 3# glass fiber honeycomb (thickness is 4 mm, the aperture of the honeycomb hole is 2.75 mm).

[0120] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 5 As shown, the reflection loss of the absorbing material prepared in this embodiment is substantially less than -10 dB at 6-18 GHz.

[0121] Example 6

[0122] It is basically the same as Example 1, with the only differences being: 1# glass fiber honeycomb (thickness is 3mm, the aperture of the honeycomb hole is 1.83mm), 2# glass fiber honeycomb (thickness is 3mm, the aperture of the honeycomb hole is 2.75mm), and 3# glass fiber honeycomb (thickness is 3mm, the aperture of the honeycomb hole is 3.67mm).

[0123] The absorbing material prepared in this embodiment was cut into a size of 300×300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 6 As shown, the reflection loss of the absorbing material prepared in this embodiment is substantially less than -10 dB in the C to Ku band (4-18 GHz).

[0124] Comparative Example 1

[0125] Preparation of microwave absorbing adhesive slurry:

[0126] 83.2g of carbon black, 2000g of medium-temperature epoxy resin, 208g of ethyl acetate, 125g of composite additive (75g of KH560 dispersant and 50g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 1# absorbing adhesive slurry;

[0127] 272.4g of carbon black, 2000g of medium-temperature epoxy resin, 523g of ethyl acetate, 136g of composite additives (82g of KH560 dispersant and 54g of Digo leveling agent) and 16.7g of curing agent were stirred and mixed at a speed of 1000r / min for 30min. After stirring, the mixture was ground three times using an S150 three-roll grinder to obtain 2# absorbing adhesive slurry.

[0128] Preparation of microwave-absorbing adhesive film: 2# microwave-absorbing adhesive slurry was coated on centrifugal paper by wet casting method with a thickness of 0.1mm. After drying in a 40℃ oven for 30min, 2# semi-cured microwave-absorbing adhesive film was obtained.

[0129] Preparation of absorbing glass fiber prepreg: using the hot melt method, place a piece of the same semi-cured absorbing adhesive film on the upper and lower sides of the glass fiber cloth, and use the calendering molding process to composite-impregnate the 2# absorbing adhesive film and the glass fiber cloth at 70°C and 0.2MPa pressure to obtain 2# absorbing glass fiber prepreg with a thickness of 0.2mm; package the absorbing glass fiber prepreg 2# in a polyethylene bag and store it in a frozen state at -18°C.

[0130] Preparation of microwave-absorbing honeycomb: After spraying 1# microwave-absorbing adhesive slurry on glass fiber honeycomb (thickness is 3mm, honeycomb hole diameter is 2.75mm), the temperature is raised to 135°C at 2°C / min and kept for 2h to solidify and form, and 1# microwave-absorbing honeycomb is obtained with a weight gain of 5%.

[0131] Laying: Laying layers on the mold in the following order from bottom to top: release cloth, reflective layer (carbon fiber prepreg) with a thickness of 0.4mm, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, 1# absorbing honeycomb, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, 1# absorbing honeycomb, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, 1# absorbing honeycomb, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, 1# absorbing honeycomb, 2# absorbing glass fiber prepreg with a thickness of 0.2mm, skin (glass fiber prepreg) with a thickness of 0.6mm, and release cloth.

[0132] Curing and molding: After the laying is completed, it is placed in a vacuum bag for evacuation (pressure is 0.1MPa), and placed in an autoclave for curing (pressure is 0.3MPa). The temperature is raised to 135℃ at a heating rate of 2℃ / min for curing. After keeping the temperature for 2h, it is cooled with the furnace. After it drops to room temperature, the vacuum pressure is released to obtain the absorbing material.

[0133] The absorbing material prepared in this comparative example was cut into a size of 300*300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 7 As shown, it can be seen that the absorbing material prepared in this comparative example has poor reflection loss performance in the range of 2 to 18 GHz, and the reflection loss basically does not reach -10 dB.

[0134] Comparative Example 2

[0135] It is basically the same as Example 1, except that the microwave-absorbing honeycomb is replaced by a glass fiber honeycomb during the laying process.

[0136] The absorbing material prepared in this comparative example was cut into a size of 300*300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Figure 8 As shown, it can be seen that the absorbing material prepared in this comparative example has poor reflection loss performance in the range of 2 to 18 GHz, and the reflection loss basically does not reach -10 dB.

[0137] Comparative Example 3

[0138] It is basically the same as Example 1, except that: during the layering process, the absorbing glass fiber prepreg is replaced by glass fiber prepreg; the difference between the glass fiber prepreg and the absorbing glass fiber prepreg is that the glass fiber prepreg does not contain carbon black.

[0139] The absorbing material prepared in this comparative example was cut into a size of 300*300 mm to be tested, and the reflectivity test was carried out according to GJB2038A-2011. The results are as follows: Fig. 9 As shown, it can be seen that the absorbing material prepared in this comparative example has poor reflection loss performance in the range of 2 to 18 GHz, and the reflection loss basically does not reach -10 dB.

[0140] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high temperature resistant structural absorbing material, characterized in that: The high temperature resistant structural absorbing material comprises a skin layer, an absorbing layer and a reflecting layer arranged in sequence from the outside to the inside along the thickness direction: The absorbing layer comprises an absorbing fiber layer and an absorbing honeycomb layer alternately arranged along the thickness direction; the dielectric loss of the absorbing fiber layer increases from the outside to the inside along the thickness direction; the raw material for preparing the absorbing fiber layer is absorbing fiber prepreg; the raw material for preparing the reflecting layer is carbon fiber prepreg; the raw material for preparing the skin layer is skin prepreg, and the skin prepreg is at least one of glass fiber prepreg and quartz fiber prepreg.

2. The high temperature resistant structural absorbing material according to claim 1, characterized in that: The raw materials for preparing the wave-absorbing fiber layer include glass fiber cloth and wave-absorbing adhesive film; and / or The raw materials for preparing the wave-absorbing honeycomb layer include fiber honeycombs and wave-absorbing adhesive slurry; preferably, the fiber honeycombs are one or more of glass fiber honeycombs and quartz fiber honeycombs.

3. The high temperature resistant structural absorbing material according to claim 2, characterized in that: The thickness of the skin layer is 0.6-0.8 mm; and / or The thickness of the reflective layer is 0.6-0.8 mm.

4. The preparation method according to claim 1, characterized in that: The honeycomb aperture of the wave-absorbing honeycomb layer decreases from the outside to the inside along the thickness direction. Preferably, the honeycomb aperture of the wave-absorbing honeycomb layer is 1 to 4 mm.

5. The preparation method according to claim 1, characterized in that: The thickness of the wave-absorbing honeycomb layer increases gradually from the outside to the inside along the thickness direction. Preferably, the thickness of the wave-absorbing honeycomb layer is 1 to 5 mm.

6. The preparation method according to claim 2, characterized in that: The absorbing adhesive slurry comprises a dielectric absorber, a binder, a solvent, a composite auxiliary agent and a curing agent; preferably, the mass ratio of the dielectric absorber, the binder, the solvent, the composite auxiliary agent and the curing agent is 2-20:80-98:10-35:2-6:0.67-0.

82.

7. The high temperature resistant structural absorbing material according to claim 6, characterized in that: The dielectric absorber is one or more of carbon black, graphene, and carbon nanotubes; The binder is one of medium-temperature epoxy resin, phenolic resin, and polyimide resin; The solvent is ethyl acetate; and / or The auxiliary agents include dispersants and leveling agents.

8. A method for preparing a high temperature resistant structural absorbing material according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: According to the performance requirements of the absorbing material, the skin prepreg, the absorbing fiber prepreg, the absorbing honeycomb layer and the carbon fiber prepreg are layered and subjected to a first curing molding to obtain a high temperature resistant structural absorbing material.

9. The preparation method according to claim 8, characterized in that: The preparation method of the absorbing fiber prepreg comprises: laminating glass fiber cloth and absorbing adhesive film, hot melting and calendering to obtain the absorbing fiber prepreg; preferably, the hot melting temperature is 65-75° C. and the pressure is 0.2-0.3 MPa.

10. The preparation method according to claim 8, characterized in that: The preparation method of the wave-absorbing honeycomb layer comprises: distributing the wave-absorbing adhesive slurry on the surface of the fiber honeycomb, and performing a second curing molding to obtain the wave-absorbing honeycomb; preferably, after curing molding, the fiber honeycomb increases in weight by 5-20%.