Preparation method and application of molybdenum-doped nickel oxide solid solution crystal and amorphous coexisting material

By using molybdenum-doped nickel oxide solid solution crystals and amorphous coexisting materials as catalysts, the impurities, complexity and high energy consumption problems of traditional H2O2 production methods are solved, and efficient and stable H2O2 production is achieved, reducing costs and energy consumption and improving Selectivity and stability of catalysts.

CN118957659APending Publication Date: 2024-11-15EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411016124.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-27
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional H2O2 production methods have impurity problems, complexity and high energy consumption, and precious metal catalysts are costly and unstable, which limits the efficiency and safety of H2 and O2 to directly synthesize H2O2.

Method used

Molybdenum-doped nickel oxide solid solution crystals and amorphous coexisting materials are used as catalysts to adjust the electronic valence state and structure of metal oxides through doping of molybdenum, optimize the catalytic activity center, reduce the catalyst cost and improve catalytic efficiency and selectivity.

Benefits of technology

It realizes efficient and stable H2O2 production, simplifies the production process, reduces costs and energy consumption, and improves the selectivity and stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957659A_ABST
    Figure CN118957659A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a molybdenum-doped nickel oxide solid solution crystal and amorphous coexisting material, and relates to the technical field of material science and engineering technology and chemistry. The preparation method comprises the specific steps that S100, raw materials are selected and mixed; the preparation method comprises the following steps: preparing raw materials: accurately weighing a certain amount of molybdenum precursor and nickel precursor, doping molybdenum and regulating crystal and non-crystal structures of nickel oxide, so that the obtained material shows higher catalytic activity and selectivity in a catalytic reaction, and the material with the structure generally has a larger specific surface area and more active sites, so that the specific surface area of the material is larger; according to the present invention, the catalyst has excellent catalytic performance in the H2O2 synthesis process through the 2e-ORR two-electron oxygen reduction reaction, such that the efficient approach is provided for the H2O2 production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of material science and engineering technology and chemical technology, and in particular to a preparation method and application of a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material. Background Art

[0002] Hydrogen peroxide H2O2, as an indispensable chemical substance, plays a vital role in many industries such as chemical, textile, electronics, medicine and environmental protection. Its unique oxidizing property makes H2O2 an indispensable raw material and intermediate in these fields. However, the current industrial production of H2O2 mainly relies on the traditional anthraquinone method. Although this method can produce H2O2 products with a concentration of up to 70wt.%, the impurity problems in its production process, the complexity brought by multi-step reactions and the high energy consumption cannot be ignored. In addition, the instability of H2O2 itself also poses challenges to its safe storage and transportation.

[0003] Then traditionally, the method of directly synthesizing H2O2 from H2 and O2 is limited in economic feasibility due to the high cost of precious metal catalysts such as platinum Pt and palladium Pd. Although the use of precious metal catalysts can achieve a higher conversion rate, the direct reaction of H2 and O2 has the risk of explosion. In addition, precious metal resources are limited and their prices fluctuate greatly. These factors limit the large-scale application of this method. In addition, although transition metal oxides have shown certain potential as potential alternative catalysts, especially their ability to synthesize H2O2 in the 2e-oxygen reduction reaction, the performance of single-component transition metal oxide catalysts still needs to be improved, especially in terms of selectivity and stability.

[0004] In summary, although H2O2 has broad application prospects in many fields, the limitations of its traditional production methods and the shortcomings of existing catalysts seriously restrict the efficiency and safety of H2O2 production. Therefore, the development of a low-cost, efficient and stable catalyst to achieve the direct synthesis of H2O2 from H2 and O2 has become a hot topic and difficulty in current research. In this context, the present invention proposes a preparation method and application of a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous solids coexist, aiming to solve the key problems in the current H2O2 production through innovative material design and synthesis strategies. Summary of the invention

[0005] The purpose of the present invention is to make up for the shortcomings of the prior art and provide a preparation method and application of a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material, which can use non-precious metals molybdenum and nickel as main components, reducing the preparation cost of the catalyst. Through molybdenum doping, the electronic valence state and structure of the metal elements in the metal oxide are adjusted, the catalytic active center is optimized, thereby improving the catalytic efficiency and product selectivity.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: On the one hand, a method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexisting material, the preparation method specifically comprises the following steps:

[0007] S100, Raw material selection and mixing:

[0008] S101, raw material preparation: accurately weigh a certain amount of molybdenum precursor and nickel precursor;

[0009] S102, adding additives: adding ammonium fluoride and urea to the mixture of molybdenum and nickel precursors according to a proportion;

[0010] S103, solvent selection and mixing: selecting a solvent, dissolving the mixture in S102 in the solvent, and ensuring uniform mixing by magnetic stirring, wherein the stirring time is controlled between 5 minutes and 24 hours;

[0011] S200, low temperature hydrothermal synthesis:

[0012] S201, hydrothermal reaction setting: transferring the mixed solution obtained in S103 to a hydrothermal reaction kettle, and setting the temperature and heating time of the hydrothermal reaction;

[0013] S202, atmosphere control: during the hydrothermal reaction, control the reaction atmosphere and set the reaction under optimal conditions;

[0014] S300, product processing:

[0015] S301, solid-liquid separation: after the hydrothermal reaction is completed, the reaction product is separated from the solvent by centrifugation and suction filtration;

[0016] S302, washing and drying: washing the separated product multiple times with the same solvent and deionized water as in S103 to remove surface residues, and placing the washed product in a drying oven until the product is completely dried;

[0017] S400, high temperature calcination:

[0018] S401, preparation before calcination: placing the dried product obtained in S302 in a calcining furnace under an inert gas atmosphere;

[0019] S402, calcination parameter setting: setting the calcination temperature, heating time and heating rate, and calcining under the optimal conditions;

[0020] S403, post-calcination treatment: After the calcination is completed, the furnace temperature is naturally reduced to room temperature, and the product is taken out to obtain a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material.

[0021] Furthermore, S101 selects a molybdenum precursor and a nickel precursor, the molybdenum precursor includes but is not limited to molybdenum chloride, molybdenum phosphide, ammonium molybdate, molybdenum fluoride, hexacarbonyl molybdenum, molybdenum boride, sodium molybdate, molybdenum sulfide, and molybdenum acetate, and the nickel precursor includes but is not limited to nickel phosphide, nickel iodide, nickel sulfide, nickel benzoate, nickel bromide, nickel acetone acetate, nickel selenide, nickel chloride, nickel hypophosphite, nickel nitrate, nickel hydroxyacetate, and nickel sulfamate.

[0022] Furthermore, in S102, the molybdenum precursor, the nickel precursor, urea and ammonium fluoride are added into the solvent and mixed evenly by magnetic stirring. The amount of urea and ammonium fluoride is 0.00001-10g, and they are mixed with the molybdenum precursor and the nickel precursor.

[0023] Furthermore, the S103 solvent includes but is not limited to water mixed with one of ethanol, ethylene glycol, acetone, chloroform, and dimethylformamide, and the magnetic stirring time is 5 minutes to 24 hours.

[0024] Furthermore, in S201, the mixed solution is subjected to a hydrothermal reaction, the hydrothermal temperature is 50-200° C., and the heating time is 30 minutes to 24 hours.

[0025] Furthermore, the S202 heating atmosphere includes but is not limited to nitrogen, hydrogen, argon, ammonia, helium, air and mixed gases. The optimal condition for the hydrothermal reaction is hydrothermal treatment at 140 degrees Celsius for 8 hours in an air atmosphere.

[0026] Furthermore, in S301, the product is separated from the reactant by centrifugation and filtration, and washed with a solvent including but not limited to water and ethanol, ethylene glycol, acetone, chloroform, and dimethylformamide, and the obtained product is placed in a drying oven and dried for 1h-24h.

[0027] Furthermore, the S402 dried product is calcined at 100-800°C, the heating time is 10 minutes-24 hours, the heating atmosphere includes but is not limited to nitrogen, hydrogen, argon, ammonia, helium, air and mixed gases, the heating rate is 0.01-500°C / min, and the optimal calcination condition is in an argon atmosphere, heating to 450°C at a heating rate of 1.4°C / min and calcining for 1 hour.

[0028] Furthermore, the coexistence material of the molybdenum-doped nickel oxide solid solution crystal and the amorphous material is used as a catalyst for catalyzing 2e -In the specific reaction process of ORR synthesis of H2O2, the catalyst can provide active sites. Oxygen molecules accept two electrons under the action of the catalyst. The active sites on the catalyst surface interact with oxygen molecules to cause a reduction reaction. Through electron transfer and the formation of chemical bonds, oxygen is gradually converted into hydrogen peroxide. In this process, the crystal and non-crystalline structures of the catalyst work together to effectively promote 2e - The ORR reaction to synthesize H2O2 proceeds.

[0029] Furthermore, the molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material in the electrocatalytic 2e - The operating conditions during the ORR synthesis of H2O2 include but are not limited to: the pH value of the electrolyte solution ranges from 1 to 14, the working potential ranges from -0.1 V to -2.0 V, and the current density ranges from 10 mA / cm 2 Up to 1000mA / cm 2 The reaction temperature ranges from 0°C to 100°C, and the reaction is carried out in a static electrolyzer, allowing O2 to diffuse to the catalyst surface.

[0030] Compared with the prior art, the preparation method and application of the molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material have the following beneficial effects:

[0031] 1. The present invention dopes and regulates the crystal and amorphous structure of nickel oxide with molybdenum, and the obtained material exhibits higher catalytic activity and selectivity in the catalytic reaction. The material with this structure usually has a larger specific surface area and more active sites, thereby improving the catalytic efficiency, which is specifically manifested in the 2e - In the process of synthesizing H2O2 via ORR (two-electron oxygen reduction reaction), the catalyst exhibited excellent catalytic performance, providing an efficient route for the production of H2O2.

[0032] 2. The preparation method of the present invention simplifies the material preparation process and reduces the complex production steps and equipment requirements by optimizing the raw material selection, hydrothermal synthesis conditions and the subsequent high-temperature calcination step. This not only makes the material production more efficient, but also reduces the production cost, which is conducive to industrial production. In addition, the use of relatively cheap and easily available raw materials and relatively low energy consumption further improves the cost-effectiveness of the method.

[0033] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 It is a scanning electron microscope image of the molybdenum-doped nickel oxide solid solution prepared by the method of the present invention.

[0036] Figure 2 It is a transmission electron microscope image of the molybdenum-doped nickel oxide solid solution prepared by the method of the present invention.

[0037] Figure 3 It is an X-ray diffraction diagram of the molybdenum-doped nickel oxide solid solution prepared by the method of the present invention.

[0038] Figure 4 It is a linear voltammetric curve diagram of the molybdenum-doped nickel oxide solid solution prepared by the method of the present invention.

[0039] Figure 5 It is the stability curve of the molybdenum-doped nickel oxide solid solution prepared by the method of the present invention. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Embodiment 1

[0042] A method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material, wherein the obtained material exhibits higher catalytic activity and selectivity in a catalytic reaction (such as an oxygen reduction reaction) by molybdenum doping and regulating the crystal and amorphous structures of nickel oxide. The steps are:

[0043] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0044] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace. Under flowing Ar, react at 450°C for 1 h (heating rate 1.4°C / min). Then, wash the brown powder alternately with deionized water and anhydrous ethanol and centrifuge it three times. Then, place the obtained brown solid in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Mo0.25Ni0.75O.

[0045] Embodiment 2

[0046] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0047] Step 1: Add 9.3048g nickel nitrate hexahydrate, 0.784g ammonium molybdate (molar ratio Mo:Ni=1:8), 1.2012g urea, and 0.2963g ammonium fluoride to 60mL deionized water and stir vigorously for 30min to obtain a uniform green solution, then transfer the solution to a 100mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0048] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace. Under flowing Ar, react at 450°C for 1 h (heating rate 1.4°C / min). Then, wash the brown powder alternately with deionized water and anhydrous ethanol and centrifuge it three times. Then, place the obtained brown solid in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Mo0.17Ni0.83O.

[0049] Embodiment 3

[0050] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0051] Step 1: Add 1.1631 g of nickel nitrate hexahydrate, 1.2012 g of urea, and 0.2963 g of ammonium fluoride to 60 mL of deionized water and stir vigorously for 30 min to obtain a uniform green solution. Then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 hours of solvothermal reaction. After the reaction is completed, cool it naturally to room temperature. Wash the product alternately with deionized water and anhydrous ethanol and centrifuge it three times, then place it in a constant temperature oven at 65°C to dry overnight.

[0052] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 450°C for 1 h (heating rate 1.4°C / min) under flowing Ar. Then, the brown powder is alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The brown solid is then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Ni0.

[0053] Embodiment 4

[0054] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0055] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0056] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 450°C in an air atmosphere for 1 h (heating rate 1.4°C / min). Then, the brown powder is alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The obtained brown solid is then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Mo0.25Ni0.75O-Air.

[0057] Embodiment 5

[0058] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0059] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0060] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 450°C for 4 hours under flowing Ar (heating rate 1.4°C / min). Then, the brown powder is alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The brown solid is then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Mo0.25Ni0.75O-4h.

[0061] Embodiment 6

[0062] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0063] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0064] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 250°C for 1 h (heating rate 1.4°C / min) under flowing Ar. Then, the brown powder was alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The brown solid was then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample was named Mo0.25Ni0.75O-250.

[0065] Embodiment 7

[0066] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0067] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0068] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 350°C for 1 h (heating rate 1.4°C / min) under flowing Ar. Then, the brown powder was alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The brown solid was then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample was named Mo0.25Ni0.75O-350.

[0069] Embodiment 8

[0070] A method for preparing a catalyst in which molybdenum-doped nickel oxide solid solution crystals and amorphous materials coexist is carried out according to the following method:

[0071] Step 1: Add 1.1631 g nickel nitrate hexahydrate, 0.784 g ammonium molybdate (molar ratio Mo:Ni=1:1), 1.2012 g urea, and 0.2963 g ammonium fluoride to 60 mL deionized water and stir vigorously for 30 min to obtain a uniform green solution, then transfer the solution to a 100 mL high-pressure reactor containing a polytetrafluoroethylene liner and place it in an oven at 140°C for 8 h of solvent thermal reaction. After the reaction is completed, it is naturally cooled to room temperature. The product is washed alternately with deionized water and anhydrous ethanol and centrifuged three times, and then placed in a constant temperature oven at 65°C to dry overnight.

[0072] Step 2: Grind the dried product thoroughly, take 30 mg and place it in a tube furnace, and react at 550°C for 1 h (heating rate 1.4°C / min) under flowing Ar. Then, the brown powder is alternately washed with deionized water and anhydrous ethanol and centrifuged three times. The brown solid is then placed in a constant temperature oven at 65°C to dry overnight. The obtained sample is named Mo0.25Ni0.75O-550.

[0073] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material, characterized in that: The specific steps of the preparation method are as follows: S100, Raw material selection and mixing: S101, raw material preparation: accurately weigh a certain amount of molybdenum precursor and nickel precursor; S102, adding additives: adding ammonium fluoride and urea to the mixture of molybdenum and nickel precursors according to a proportion; S103, solvent selection and mixing: selecting a solvent, dissolving the mixture in S102 in the solvent, and ensuring uniform mixing by magnetic stirring, wherein the stirring time is controlled between 5 minutes and 24 hours; S200, low temperature hydrothermal synthesis: S201, hydrothermal reaction setting: transferring the mixed solution obtained in S103 to a hydrothermal reaction kettle, and setting the temperature and heating time of the hydrothermal reaction; S202, atmosphere control: during the hydrothermal reaction, control the reaction atmosphere and set the reaction under optimal conditions; S300, product processing: S301, solid-liquid separation: after the hydrothermal reaction is completed, the reaction product is separated from the solvent by centrifugation and suction filtration; S302, washing and drying: washing the separated product multiple times with the same solvent and deionized water as in S103 to remove surface residues, and placing the washed product in a drying oven until the product is completely dried; S400, high temperature calcination: S401, preparation before calcination: placing the dried product obtained in S302 in a calcination furnace under an inert gas atmosphere; S402, calcination parameter setting: setting the calcination temperature, heating time and heating rate, and calcining under the optimal conditions; S403, post-calcination treatment: After the calcination is completed, the furnace temperature is naturally lowered to room temperature, and the product is taken out to obtain a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material.

2. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The S101 selects a molybdenum precursor and a nickel precursor, the molybdenum precursor includes but is not limited to molybdenum chloride, molybdenum phosphide, ammonium molybdate, molybdenum fluoride, molybdenum hexacarbonyl, molybdenum boride, sodium molybdate, molybdenum sulfide, and molybdenum acetate; the nickel precursor includes but is not limited to nickel phosphide, nickel iodide, nickel sulfide, nickel benzoate, nickel bromide, nickel acetone acetate, nickel selenide, nickel chloride, nickel hypophosphite, nickel nitrate, nickel hydroxyacetate, and nickel sulfamate.

3. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 2, characterized in that: In the step S102, a molybdenum precursor, a nickel precursor, urea and ammonium fluoride are added into a solvent and mixed evenly by magnetic stirring. The amount of urea and ammonium fluoride is 0.00001-10 g, and the urea and ammonium fluoride are mixed with the molybdenum precursor and the nickel precursor.

4. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The S103 solvent includes but is not limited to water mixed with one of ethanol, ethylene glycol, acetone, chloroform, and dimethylformamide, and the magnetic stirring time is 5 minutes to 24 hours.

5. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: In S201, the mixed solution is subjected to a hydrothermal reaction, the hydrothermal temperature is 50-200° C., and the heating time is 30 minutes to 24 hours.

6. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The S202 heating atmosphere includes but is not limited to nitrogen, hydrogen, argon, ammonia, helium, air and mixed gases. The optimal condition for the hydrothermal reaction is hydrothermal reaction at 140 degrees Celsius for 8 hours in an air atmosphere.

7. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: In S301, the product is separated from the reactant by centrifugation and filtration, and washed with a solvent including but not limited to water and ethanol, ethylene glycol, acetone, chloroform, and dimethylformamide. The obtained product is placed in a drying oven and dried for 1h-24h.

8. The method for preparing a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The S402 dried product is calcined at 100-800°C for 10 minutes to 24 hours. The heating atmosphere includes but is not limited to nitrogen, hydrogen, argon, ammonia, helium, air and mixed gases. The heating rate is 0.01-500°C / min. The optimal calcination condition is to heat the temperature to 450°C for 1 hour in an argon atmosphere at a heating rate of 1.4°C / min.

9. The use of a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The coexistence material of the molybdenum-doped nickel oxide solid solution crystal and the amorphous material is used as a catalyst for catalyzing 2e - In the specific reaction process of ORR synthesis of H2O2, the catalyst can provide active sites. Oxygen molecules accept two electrons under the action of the catalyst. The active sites on the catalyst surface interact with oxygen molecules to undergo a reduction reaction. Through electron transfer and the formation of chemical bonds, oxygen is gradually converted into hydrogen peroxide. In this process, the crystal and non-crystalline structures of the catalyst work together to effectively promote 2e - The ORR reaction to synthesize H2O2 proceeds.

10. The use of a molybdenum-doped nickel oxide solid solution crystal and amorphous coexistence material according to claim 1, characterized in that: The operating conditions of the molybdenum-doped nickel oxide solid solution crystal and amorphous coexisting material in the electrocatalytic 2e-ORR synthesis of H2O2 include but are not limited to: the pH value of the electrolyte solution ranges from 1 to 14, the working potential ranges from -0.1 V to -2.0 V, and the current density ranges from 10 mA / cm 2 Up to 1000mA / cm 2 The reaction temperature ranges from 0°C to 100°C, and the reaction is carried out in a static electrolyzer, allowing O2 to diffuse to the catalyst surface.

Citation Information

Cited By

  • Li / Na ion battery negative electrode material heterojunction and construction method and performance prediction method thereof

    CN122068008A