Wool-like polyester production method and fabric

By using the ups and downs and floating interweaving and specific chemical treatment of thick and detailed polyester fibers, a wool-like polyester fabric with a wool-like touch and appearance is formed, which solves the problems of high cost and limited application range in the existing technology, and achieves low-cost production and wide application. effect.

CN118957840APending Publication Date: 2024-11-15NANTONG TEIJIN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411276206.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the preparation of imitation wool fabrics with polyester fabrics is high in cost and has a limited range of applications, making it difficult to produce fabrics with a wool-like feel and suitable for a variety of environments at low cost.

Method used

Coarse and fine polyester fibers are used for ups and downs and interwoven, combined with NaOH solution, refining agent and chelating agent, and after the pre-setting, reduction and post-setting, fabrics with regular reduction amplitude and crystallinity are formed, reducing production costs and increasing production costs. Applicability of fabric.

Benefits of technology

It has achieved low-cost production of imitation wool polyester fabrics, with a wool-like touch and appearance, suitable for a variety of environments, comfortable to wear, and has broad market application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957840A_ABST
    Figure CN118957840A_ABST
Patent Text Reader

Abstract

The invention discloses a wool-like polyester production method and a fabric, relates to the technical field of textile dyeing and finishing, and provides a wool-like polyester production method and a fabric which have wool-like touch feeling and appearance, are suitable for various environments and are easy to care. The method comprises the following steps: S1, weaving; the yarns are slub polyester fibers, and are interwoven up and down to form gray cloth; s2, carrying out pretreatment; adding a NaOH solution, a scouring agent and a chelating agent into a bath solution of the desizing machine to treat the fabric; s3, drying; performing drying treatment on the fabric; s4, performing pre-shaping; heat setting processing is carried out, the processing temperature is 180 DEG C, and the processing speed is 30 m / min; s5, reduction is carried out; the concentration of the NaOH solution in an alkali tank of the decrement machine is set to be 23-29 baume degrees, and the residence time of the fabric in a steam box of the decrement machine is set to be 5 min; s6, post-shaping; and heat setting processing is carried out, the processing temperature is 150-170 DEG C, and the processing speed is 30 m / min.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile dyeing and finishing, and in particular to a wool-like polyester production method and fabric. Background Art

[0002] Wool fabrics have the advantages of being soft to the touch and comfortable, but at the same time, they also generally have defects such as being relatively expensive, highly hygroscopic, not suitable for humid environments, and requiring special care.

[0003] There are technical attempts in the prior art to prepare wool-like fabrics from polyester fabrics, but such technical solutions have extremely high requirements on yarns, the production cost of the fabrics remains high, and the scope of application is relatively limited.

[0004] Therefore, how to improve the dyeing and finishing process of polyester fabrics and prepare polyester wool-like fabrics at low cost has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a method for producing imitation wool polyester and a fabric which has a wool-like touch and appearance, is suitable for a variety of environments, and is easy to care for.

[0006] The technical solution of the present invention is: A method for producing a wool-like polyester fabric comprises the following steps: S1: Weaving; the yarn is made of coarse and fine polyester fibers, and the yarn is interwoven into a grey cloth using a loom; S2: Pretreatment: adding NaOH solution, scouring agent and chelating agent to the slurry of the desizing machine to treat the fabric, remove the sizing agent and oil in the fabric, and pre-shrink the fabric; S3: Drying: Use a dryer to dry the fabric; S4: Pre-setting; use a setting machine for heat setting processing, the processing temperature is 180℃, and the processing speed is 30m / min; S5: weight reduction; the fabric is weight reduced by using NaOH solution, the concentration of NaOH solution in the alkali tank of the weight reduction machine is set to 23-29 degrees Baume, and the residence time of the fabric in the steam box of the weight reduction machine is set to 5 minutes; S6: Post-setting: Use a setting machine for heat setting processing, the processing temperature is 150-170°C, and the processing speed is 30m / min.

[0007] In the step S5, the reduction rate of the fabric is 16-25%.

[0008] The coarse and fine polyester fibers are two-component polyester long fibers, and the difference in characteristic viscosity between the two components of the two-component polyester long fibers is greater than 0.4 dl / g.

[0009] The bath temperature of the alkali bath in step S5 is 105°C.

[0010] In the step S2, the concentration of the NaOH solution is 32%, the dosage is 2 g / L, the dosage of the scouring agent is 1.5 g / L, and the dosage of the chelating agent is 1.5 g / L.

[0011] In the step S2, the processing temperature is 95° C. and the processing speed is 50 m / min.

[0012] A wool-like polyester fabric is produced according to the production method of the wool-like polyester fabric.

[0013] The fabric is double-faced plain.

[0014] The width of the fabric is 100 to 300 cm.

[0015] The wool-like polyester production method of the present invention forms regular and differential fiber processing characteristics such as reduction amplitude, shrinkage and crystallinity in the length direction of coarse and fine fibers through a unique polyester fiber dyeing and finishing process. The prepared fabric is elastic, delicate in hand, has a wool-like touch and appearance, and can greatly reduce the production cost of the wool-like fabric.

[0016] The wool-like polyester fabric of the present invention not only meets consumers' demand for fabrics with wool-like touch and appearance, but also has advantages that traditional wool fabrics do not have, such as being suitable for a variety of environments, easy to care for, and comfortable to wear, and has broad market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of a process for producing a wool-like polyester fabric of the present invention. Figure 2 It is a schematic diagram of the structure of coarse and fine polyester fibers in a method for producing a wool-like polyester fabric of the present invention. Figure 3 The present invention is a structural schematic diagram of a wool-like polyester fabric. DETAILED DESCRIPTION

[0018] The following is combined with Figure 1-3 , further illustrating the present invention.

[0019] The invention discloses a method for producing a wool-like polyester fabric, comprising the following steps: S1: weaving; the yarn adopts coarse and fine polyester fibers, which are usually prepared by an uneven drafting process; the yarns in the warp direction and the yarns in the weft direction are interwoven into a grey cloth by a loom. S2: pre-treatment; the fabric is treated by adding a NaOH solution, a scouring agent and a chelating agent to the trough liquid of a desizing machine, the sizing agent and the oil agent in the fabric are removed, and the fabric is pre-shrunk to make the surface of the fabric smooth. S3: drying; the fabric is dried by a dryer to improve the structural stability of the fabric and ensure that the fabric properties are uniform in subsequent processing. S4: pre-setting; the setting machine is used for heat setting processing, the processing temperature is 180°C, and the processing speed is 30m / min, which is used to eliminate wrinkles on the fabric. S5: reduction; the fabric is reduced by using a NaOH solution, the concentration of the NaOH solution in the alkali tank of the reduction machine is set to 23-29 degrees Baume; the retention time of the fabric in the steam box of the reduction machine is set to 5min. According to customer needs, the fabric after weight reduction treatment can be dyed. The dyeing temperature is about 135℃ and the time is about 30min. 2g / L of 32% NaOH solution, 1.2g / L of leveling agent and dye required according to color requirements are added to the dye liquor. The fabric can also be resin treated after dyeing to make the fabric have better sweat absorption performance. S6: Post-setting; use a setting machine for heat setting processing, the processing temperature is 150-170℃, the processing speed is 30m / min, which is used to eliminate fabric wrinkles and ensure the stability of fabric size. See Figure 2 , coarse and fine polyester fibers have coarse and fine parts in the length direction. The coarse and fine parts will have differences in reduction, shrinkage, crystallinity, dyeability, etc. in the subsequent unique dyeing and finishing processing. These differential processing characteristics make the fabric different from ordinary polyester fiber fabrics, soft, fluffy, elastic, and delicate in feel, making it have a touch and appearance close to wool fabrics. See the fabric structure diagram for details. Figure 3 The elastic elongation of the fabric prepared by the present invention is 5% to 50%, the elastic recovery rate is greater than 70%, the tear strength of the fabric in the warp and weft directions is greater than 6N, and the gram weight is 30 to 500g / ㎡.

[0020] In step S5, the weight reduction rate of the fabric is 16-25%.

[0021] The coarse and fine polyester fibers are two-component polyester long fibers, which can be either regenerated fibers or non-regenerated fibers; the gloss of the fibers can be any one or a combination of full matte, semi-matte, and glossy; the characteristic viscosity difference between the two components of the two-component polyester long fibers is greater than 0.4dl / g, and the greater the viscosity difference, the better the elasticity of the fabric.

[0022] The bath temperature of the alkali bath in step S5 is 105°C.

[0023] In step S2, the concentration of NaOH solution is 32%, the dosage is 2 g / L, the dosage of scouring agent is 1.5 g / L, and the dosage of chelating agent is 1.5 g / L.

[0024] In step S2, the processing temperature is 95° C. and the processing speed is 50 m / min.

[0025] The invention discloses an imitation wool polyester fabric, which is prepared according to a production method of the imitation wool polyester fabric.

[0026] The fabric is double-faced plain.

[0027] The width of the fabric is 100 to 300 cm.

[0028] Example 1: Using two-component unevenly drawn polyester FDY filament as yarn, setting the upper machine width to 200cm, and weaving a double-sided plain fabric with a loom, wherein the characteristic viscosities of the two components in the two-component unevenly drawn polyester FDY filament are 0.88dl / g and 0.46dl / g respectively. Use a desizing machine for pre-treatment processing, the processing temperature is 95℃, and the processing speed is 50m / min; add 2g / L of 32% concentration NaOH solution, 1.5g / L of scouring agent, and 1.5g / L of chelating agent to the tank liquid of the desizing machine to remove the sizing agent and oil in the fabric, and make it fully shrink, and the fabric surface is flat. Set the dryer temperature to 125℃ and the speed to 30m / min to dry the fabric. Perform a pre-setting treatment on the fabric at a temperature of 180℃ and a processing speed of 30m / min to eliminate the wrinkles of the fabric. The pre-shaped fabric is subjected to a weight reduction treatment by a weight reduction machine. Water is poured into the alkali tank of the weight reduction machine and NaOH is added so that the concentration of the NaOH solution is 23 degrees Baume and the temperature is 105°C. The speed of the fabric passing through the alkali tank is set to 30m / min; the retention time of the fabric in the steam box of the weight reduction machine is set to 5min; the fabric weight reduction rate is controlled to 16%. Heat setting treatment is carried out at a temperature of 170°C and a processing speed of 30m / min to eliminate wrinkles on the fabric and ensure the stability of the fabric size. The fabric prepared in this embodiment has good elasticity, and its visual similarity to the appearance of wool fabric is: relatively similar.

[0029] Example 2: Using two-component unevenly drawn polyester FDY filament as yarn, setting the upper machine width to 200cm, and weaving a double-sided plain fabric with a loom, wherein the characteristic viscosities of the two components in the two-component unevenly drawn polyester FDY filament are 0.88dl / g and 0.46dl / g respectively. Use a desizing machine for pre-treatment processing, the processing temperature is 95℃, and the processing speed is 50m / min; add 2g / L of 32% concentration NaOH solution, 1.5g / L of scouring agent, and 1.5g / L of chelating agent to the tank liquid of the desizing machine to remove the sizing agent and oil in the fabric, and make it fully shrink, and the fabric surface is flat. Set the dryer temperature to 125℃ and the speed to 30m / min to dry the fabric. Perform a pre-setting treatment on the fabric at a temperature of 180℃ and a processing speed of 30m / min to eliminate the wrinkles of the fabric. The pre-set fabric is subjected to a weight reduction treatment by a weight reduction machine. Water is injected into the alkali tank of the weight reduction machine and NaOH is added so that the concentration of the NaOH solution is 29 degrees Baume and the temperature is 105°C. The speed of the fabric passing through the alkali tank is set to 30m / min; the retention time of the fabric in the steam box of the weight reduction machine is set to 5min; the fabric weight reduction rate is controlled to 25%. A heat setting treatment is performed at a temperature of 160°C and a processing speed of 30m / min to eliminate wrinkles in the fabric and ensure the stability of the fabric size. The fabric prepared in this embodiment has good elasticity, and the visual evaluation shows that the appearance of the fabric is very similar to that of the wool fabric.

[0030] Example 3: Using two-component unevenly drawn polyester FDY filament as yarn, setting the upper machine width to 100 cm, and weaving a double-sided plain fabric with a loom, wherein the characteristic viscosities of the two components in the two-component unevenly drawn polyester FDY filament are 1.02 dl / g and 0.46 dl / g, respectively. Use a desizing machine for pre-treatment, with a processing temperature of 95°C and a processing speed of 50 m / min; add 2 g / L of 32% NaOH solution, 1.5 g / L of scouring agent, and 1.5 g / L of chelating agent to the tank liquid of the desizing machine to remove the sizing agent and oil in the fabric, and make it fully shrink, and the fabric surface is flat. Set the dryer temperature to 125°C and the speed to 30 m / min to dry the fabric. Perform a pre-setting treatment on the fabric at a temperature of 180°C and a processing speed of 30 m / min to eliminate the wrinkles of the fabric. The pre-set fabric is subjected to a weight reduction treatment by a weight reduction machine. Water is injected into the alkali tank of the weight reduction machine and NaOH is added so that the concentration of the NaOH solution is 23 degrees Baume and the temperature is 105°C. The speed of the fabric passing through the alkali tank is set to 30m / min; the retention time of the fabric in the steam box of the weight reduction machine is set to 5min; the fabric weight reduction rate is controlled to 16%. A heat setting treatment is performed at a temperature of 160°C and a processing speed of 30m / min to eliminate wrinkles in the fabric and ensure the stability of the fabric size. The fabric prepared in this embodiment has good elasticity, and its appearance similarity to the wool fabric is visually evaluated: relatively similar.

[0031] Example 4: Using 100% of two-component unevenly drawn polyester FDY filament as yarn, setting the upper machine width to 400cm, and weaving a double-sided plain fabric with a loom, wherein the characteristic viscosities of the two components in the two-component unevenly drawn polyester FDY filament are 1.33dl / g and 0.46dl / g, respectively. Use a desizing machine for pre-treatment processing, the processing temperature is 95°C, and the processing speed is 50m / min; add 2g / L of 32% concentration NaOH solution, 1.5g / L of scouring agent, and 1.5g / L of chelating agent to the tank liquid of the desizing machine to remove the sizing agent and oil in the fabric, and make it fully shrink, and the fabric surface is flat. Set the dryer temperature to 125°C and the speed to 30m / min to dry the fabric. Perform a pre-setting treatment on the fabric at a temperature of 180°C and a processing speed of 30m / min to eliminate the wrinkles of the fabric. The pre-shaped fabric is subjected to a weight reduction treatment by a weight reduction machine. Water is injected into the alkali tank of the weight reduction machine and NaOH is added so that the concentration of the NaOH solution is 25 degrees Baume and the temperature is 105°C. The speed of the fabric passing through the alkali tank is set to 30m / min; the residence time of the fabric in the steam box of the weight reduction machine is set to 5min; the fabric weight reduction rate is controlled to 20%. Heat setting treatment is carried out at a temperature of 150°C and a processing speed of 30m / min to eliminate wrinkles on the fabric and ensure the stability of the fabric size. The fabric prepared in this embodiment has excellent elasticity. Visual evaluation shows that its appearance is similar to that of wool fabric: relatively similar.

[0032] Comparative Example: Ordinary polyester fiber is used as yarn, the upper machine width is set to 200cm, and the double-sided plain fabric is woven by a loom. Use a desizing machine for pre-treatment, the processing temperature is 95℃, and the processing speed is 50m / min; add 2g / L of 32% concentration NaOH solution, 1.5g / L of scouring agent, and 1.5g / L of chelating agent to the tank liquid of the desizing machine to remove the sizing and oil in the fabric, and make it fully shrink, and the surface of the fabric is flat. Set the dryer temperature to 125℃ and the speed to 30m / min to dry the fabric. Pre-set the fabric at a temperature of 180℃ and a processing speed of 30m / min to eliminate the wrinkles of the fabric. Heat setting treatment is carried out at a temperature of 160℃ and a processing speed of 30m / min to eliminate the wrinkles of the fabric and ensure the stability of the fabric size. The fabric obtained in the comparative example has average elasticity, and its visual evaluation of the similarity of appearance with wool fabric is: not similar.

[0033] Regarding the contents disclosed in the present invention, there are still the following points to be explained: (1) The embodiments disclosed in the present invention are only examples, and the technical solutions implemented by other equivalent alternative technical means shall fall within the protection scope of the present invention; (2) In the absence of conflict, the technical features disclosed in the present invention may be combined with each other to obtain new embodiments; The above are only specific implementation methods disclosed in the present invention, but the protection scope of the present invention is not limited thereto. Technical solutions obtained after modifications and transformations of certain technical features by those skilled in the art based on the contents disclosed in the present invention should all be within the protection scope of the present invention.

Claims

1. A method for producing a wool-like polyester fabric, characterized in that: The following steps are involved: S1: Weaving; the yarn is made of coarse and fine polyester fibers, and the yarn is interwoven into a grey cloth using a loom; S2: Pretreatment: adding NaOH solution, scouring agent and chelating agent to the slurry of the desizing machine to treat the fabric, remove the sizing agent and oil in the fabric, and pre-shrink the fabric; S3: Drying: Use a dryer to dry the fabric; S4: Pre-setting; use a setting machine for heat setting processing, the processing temperature is 180℃, and the processing speed is 30m / min; S5: weight reduction; the fabric is weight reduced by using NaOH solution, the concentration of NaOH solution in the alkali tank of the weight reduction machine is set to 23-29 degrees Baume, and the residence time of the fabric in the steam box of the weight reduction machine is set to 5 minutes; S6: Post-setting: Use a setting machine for heat setting processing, the processing temperature is 150-170°C, and the processing speed is 30m / min.

2. The method for producing a wool-like polyester fabric according to claim 1, characterized in that: In the step S5, the reduction rate of the fabric is 16-25%.

3. The method for producing a wool-like polyester fabric according to claim 1, characterized in that: The coarse and fine polyester fibers are two-component polyester long fibers, and the difference in characteristic viscosity between the two components of the two-component polyester long fibers is greater than 0.4 dl / g.

4. The method for producing a wool-like polyester fabric according to claim 1, characterized in that: The bath temperature of the alkali bath in the step S5 is 105°C.

5. The method for producing a wool-like polyester fabric according to claim 1, characterized in that: In the step S2, the concentration of the NaOH solution is 32%, the dosage is 2 g / L, the dosage of the scouring agent is 1.5 g / L, and the dosage of the chelating agent is 1.5 g / L.

6. The method for producing a wool-like polyester fabric according to claim 5, characterized in that: In the step S2, the processing temperature is 95° C. and the processing speed is 50 m / min.

7. A wool-like polyester fabric, characterized in that: The method for producing a wool-like polyester fabric according to any one of claims 1 to 6 is used.

8. The imitation wool polyester fabric according to claim 7, characterized in that: The fabric is double-faced plain.

9. The imitation wool polyester fabric according to claim 7, characterized in that: The width of the fabric is 100 to 300 cm.

Citation Information

Patent Citations

  • Elastic fabric and production method thereof

    CN104420058A

  • Worsted-like cloth and producing method thereof

    CN1537184A

  • Method for manufacturing textile and textile fabric manufactured by thereof

    KR1020090011653A

  • Yarn having a basis of polyester with irregular titer

    US3958406A