UV (ultraviolet) curing material for trenchless repair of pipeline and glass fiber cloth soaked with UV curing material

By combining unsaturated polyester resin containing long soft bond segments with surface-treated glass fibers in UV cured non-excavation pipeline repair materials, the problem of insufficient material bonding is solved and pipeline repair is improved The strength and toughness of the material achieve efficient pipeline repair effect.

CN118978644APending Publication Date: 2024-11-19SHANGHAI GRANCOM TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202311315651.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Among the existing UV cured non-excavation pipeline repair materials, the bonding properties of resin and glass fiber reinforced materials are insufficient, resulting in a decrease in bonding force and strength between pipelines, affecting service life, and the stiffness of glass fiber reinforced materials is more than resistant to wear, It has insufficient flexibility, acid resistance and water resistance, and is not suitable for long-distance transportation pipeline repair.

Method used

Unsaturated polyester resin containing silane coupling agent with long soft bond segments is combined with surface-treated glass fibers to improve the bonding tightness of the resin and glass fibers, and enhance the use of specific component ratios and surface treatment agents. The material has both strength and toughness.

Benefits of technology

It significantly improves the interlayer bonding and overall performance of pipeline repair materials, enhances the bending strength, bending modulus, tensile strength and bonding strength to steel sheets, ensures the high strength, stiffness and sealing of the pipeline after repair, and can It independently withstands internal and external pressure and has a stable repair effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of trenchless pipeline repair, and particularly discloses a UV curing material for trenchless pipeline repair and glass fiber cloth soaked with the UV curing material. The invention relates to a UV curing material for trenchless repair of pipelines. The UV curing material comprises unsaturated polyester resin, a diluent, a photosensitizer, a thickener, a coupling agent and a defoaming agent, the unsaturated polyester resin is a linear high-molecular compound which is formed by polycondensation of unsaturated dibasic acid and dihydric alcohol and has ester bonds and unsaturated double bonds; the coupling agent is a mixture of gamma-aminopropyltriethoxysilane and hydrocarbyl triethoxysilane with the hydroxyl carbon atom number larger than or equal to 6, and the weight ratio of the gamma-aminopropyltriethoxysilane to the hydrocarbyl triethoxysilane is 1: (1.4-1.6). The problem of bonding between the UV curing resin and the glass fiber reinforced material is solved, the adherence between glass fiber layers is improved, and a pipeline with both strength and toughness can be obtained when the glass fiber reinforced composite material is applied to trenchless pipeline repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of trenchless pipeline repair, and more particularly to a UV curing material for trenchless pipeline repair and a glass fiber cloth impregnated with the UV curing material. Background Art

[0002] The total length of my country's buried water pipelines exceeds 4 million kilometers, and many of them are over 20 years old, and are generally old and in need of repair. Due to changes in urban construction, in many cases, old and defective pipelines cannot be repaired or replaced, so they can only be ① scrapped and decommissioned; ② used with defects; ③ repaired without trenching.

[0003] Trenchless repair is a pipeline repair technology introduced from abroad in recent years and gradually emerging in China. It is widely promoted because of its less damage to sewage pipes, high construction and repair efficiency, and less material consumption. Among them, the in-situ curing method (CIPP) trenchless repair process is the most effective and adaptable trenchless repair technology. CIPP method currently has two routes: UV curing and thermal curing. UV curing trenchless pipeline repair technology has been rapidly developed and applied due to its advantages such as fast repair speed, high repair quality, stable and reliable, and short construction plugging time.

[0004] Existing UV-curable trenchless pipeline repair materials are mainly composed of resin and glass fiber reinforced materials. However, the existing materials often have insufficient interface bonding between the resin and the glass fiber reinforced materials, resulting in the formation of voids, which reduces the interlayer bonding force and strength of the pipeline, which will affect the service life of the pipeline and even cause cracking and deformation of the pipeline. In addition, the glass fiber reinforced materials used in the above-mentioned prior art have excessive rigidity, but relatively insufficient wear resistance, flexibility, acid resistance and water resistance, and are not suitable for use as reinforcement materials for long-distance transmission pipeline repair materials. Summary of the invention

[0005] In order to solve the problem of bonding between UV curing resin and glass fiber reinforced material, improve the adhesion between glass fiber layers, and obtain a pipeline with both strength and toughness, the present application provides a UV curing material for non-excavation repair of pipelines and a glass fiber cloth impregnated with the UV curing material. A silane coupling agent containing a long soft bond segment is added to the resin formula in the present application, which improves the tightness of bonding between the resin and the glass fiber reinforced material, and the glass fiber is surface treated and has a silane coupling agent on the surface, so it can be well bonded with the resin.

[0006] In the first aspect, the present application provides a UV curing material for trenchless pipeline repair, which adopts the following technical solution: A UV curing material for trenchless pipeline repair, comprising the following components in parts by weight: Unsaturated polyester resin 50-80 parts; 10-40 parts of diluent; Photosensitizer 0.1-0.7 parts; Thickener 1-10 parts; Coupling agent 0.1-3 parts; Defoaming agent 0.1-2 parts; The unsaturated polyester resin is a linear polymer compound having an ester bond and an unsaturated double bond formed by polycondensation of an unsaturated dibasic acid and a diol; The unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to nadic anhydride is (0.4-0.6):1; The diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is (1.5-2.5):1; The coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 is 1:(1.4-1.6).

[0007] Preferably, the unsaturated dibasic acid is composed of fumaric anhydride and nadic anhydride in a weight ratio of 0.5:1; The diol is composed of neopentyl glycol and 1,2-propylene glycol in a weight ratio of 2:1.

[0008] Preferably, the preparation method of the unsaturated polyester resin is: in an inert atmosphere, a diol and an unsaturated dibasic acid are subjected to a condensation polymerization reaction under the catalytic action of a catalyst, and then a capping agent is added for capping to obtain an unsaturated polyester resin; Wherein, the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the end-capping agent is 1:(1.4-1.6):(0.05-0.08):(0.1-0.2).

[0009] Preferably, the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the end-capping agent is 1:1.5:0.06:0.15.

[0010] Preferably, the weight ratio of the γ-aminopropyltriethoxysilane to the hydrocarbon triethoxysilane having 6 or more hydroxyl carbon atoms is 1:1.5.

[0011] Preferably, the hydrocarbyl triethoxysilane having 6 or more hydroxyl carbon atoms is octyl triethoxysilane.

[0012] In a second aspect, the present application provides a glass fiber cloth impregnated with the UV curing material in the first aspect, using the following technical solution: A glass fiber cloth, wherein the weight ratio of the UV curing material used for trenchless repair of pipelines to the glass fiber cloth is (0.3-0.7):1.

[0013] Preferably, the glass fiber cloth is a surface-treated E-cR glass fiber cloth, and the surface treatment method of the E-cR glass fiber cloth is: spraying surface treatment agent I and surface treatment agent II on the surface of the glass fiber cloth in sequence, and drying to obtain the glass fiber cloth; The surface treatment agent I is composed of 0.5-1wt% of a silane coupling agent, 0.4-0.6wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 3 using a pH adjuster before use; The surface treatment agent II is composed of 3-5wt% of a silane coupling agent, 1.5-2wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 5 with a pH adjuster before use.

[0014] Preferably, the surfactants in the surface treatment agent I and the surface treatment agent II are both silicone nonionic surfactants; The silane coupling agents in the surface treatment agent I and the surface treatment agent II are both composed of a mixture of gamma-aminopropyltriethoxysilane and octyltriethoxysilane in a weight ratio of 1:(0.3-0.5). Implementation

[0015] In order to make the purpose, technical scheme and technical effect of the embodiment of the present application clearer, the technical scheme of the embodiment of the present application will be clearly and completely described below. It is worth noting that the described embodiments are only some embodiments of the present application, not all embodiments. Based on the described embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0016] Unless otherwise defined, the technical terms or scientific terms used herein shall have the common meanings understood by persons with ordinary skills in the field to which this application belongs. The words "one" or "an" and the like used in the patent application specification and claims of this application do not indicate a quantity limitation, but indicate the existence of at least one.

[0017] The raw materials used in the examples of the present application are commercially available unless otherwise specified. Example

[0018] A UV curing material for trenchless pipeline repair, wherein the raw materials used for preparing the UV curing material are: 50 kg of unsaturated polyester resin, 10 kg of diluent, 0.1 kg of photosensitizer, 1 kg of thickener, 0.1 kg of coupling agent, and 0.1 kg of defoaming agent.

[0019] The unsaturated polyester resin is a linear polymer compound having an ester bond and an unsaturated double bond formed by polycondensation of an unsaturated dibasic acid and a diol, wherein the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.4:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 1.5:1; The preparation method of the unsaturated polyester resin comprises: in an inert atmosphere, carrying out a polycondensation reaction of a diol and an unsaturated dibasic acid under the catalytic action of a catalyst (dibutyltin dilaurate), and then adding a capping agent (pentaerythritol triallyl ether) for capping to obtain the unsaturated polyester resin; wherein the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the capping agent is 1:1.4:0.05:0.1; The photosensitizer is benzoin dimethyl ether; The diluent is ethoxylated trimethylolpropane triacrylate; The thickener is Luvatol MK 25 thickener; The defoamer is BYK-066N; The coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane (octyltriethoxysilane) with hydroxyl carbon atoms ≥6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 is 1:1.4. Example

[0020] A UV curing material for trenchless pipeline repair, which is different from Example 1 in that the raw materials used in its preparation are: 75 kg of unsaturated polyester resin, 25 kg of diluent, 0.4 kg of photosensitizer, 5.5 kg of thickener, 1.5 kg of coupling agent, and 1 kg of defoaming agent. Example

[0021] A UV curing material for trenchless pipeline repair, which is different from Example 1 in that the raw materials used in its preparation are: 80 kg of unsaturated polyester resin, 40 kg of diluent, 0.7 kg of photosensitizer, 10 kg of thickener, 3 kg of coupling agent, and 2 kg of defoaming agent. Example

[0022] A UV curing material for trenchless pipeline repair, which is different from Example 1 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 1.5:1. Example

[0023] A UV curing material for trenchless pipeline repair, which is different from Example 1 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.6:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 1.5:1. Example

[0024] A UV curing material for trenchless pipeline repair, which is different from Example 4 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2:1. Example

[0025] A UV curing material for trenchless pipeline repair, which is different from Example 4 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2.5:1. Example

[0026] A UV curing material for trenchless pipeline repair, which is different from Example 6 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2:1.

[0027] The preparation method of the unsaturated polyester resin is as follows: in an inert atmosphere, diol and unsaturated dibasic acid are subjected to condensation polymerization under the catalytic action of a catalyst (dibutyltin dilaurate), and then a capping agent (pentaerythritol triallyl ether) is added for capping to obtain the unsaturated polyester resin; wherein the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the capping agent is 1:1.5:0.06:0.15. Example

[0028] A UV curing material for trenchless pipeline repair, which is different from Example 6 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2:1.

[0029] The preparation method of the unsaturated polyester resin is as follows: in an inert atmosphere, diol and unsaturated dibasic acid are subjected to condensation polymerization under the catalytic action of a catalyst (dibutyltin dilaurate), and then a capping agent (pentaerythritol triallyl ether) is added for capping to obtain the unsaturated polyester resin; wherein the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the capping agent is 1:1.6:0.08:0.2. Example

[0030] A UV curing material for trenchless pipeline repair, which is different from Example 8 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2:1.

[0031] The preparation method of the unsaturated polyester resin comprises: in an inert atmosphere, carrying out a polycondensation reaction of a diol and an unsaturated dibasic acid under the catalytic action of a catalyst (dibutyltin dilaurate), and then adding a capping agent (pentaerythritol triallyl ether) for capping to obtain the unsaturated polyester resin; wherein the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the capping agent is 1:1.5:0.06:0.15; The coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 (octyltriethoxysilane), wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 is 1:1.5. Example

[0032] A UV curing material for trenchless pipeline repair, which is different from Example 8 in that: Among them, the unsaturated polyester resin is a linear polymer compound with ester bonds and unsaturated double bonds formed by the condensation of unsaturated dibasic acid and diol, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to methyl methacrylate anhydride is 0.5:1; the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 2:1.

[0033] The preparation method of the unsaturated polyester resin comprises: in an inert atmosphere, carrying out a polycondensation reaction of a diol and an unsaturated dibasic acid under the catalytic action of a catalyst (dibutyltin dilaurate), and then adding a capping agent (pentaerythritol triallyl ether) for capping to obtain the unsaturated polyester resin; wherein the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the capping agent is 1:1.5:0.06:0.15; The coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane (octyltriethoxysilane) with hydroxyl carbon atoms ≥6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 is 1:1.6.

[0034] Application Example 1-11 The UV curing materials for trenchless pipeline repair obtained in Examples 1-11 were respectively impregnated into glass fiber cloth to obtain the same.

[0035] The weight ratio of UV curing material to fiberglass cloth used for trenchless pipe repair is 0.3:1.

[0036] The glass fiber cloth is a surface-treated E-cR glass fiber cloth, and the surface treatment method of the E-cR glass fiber cloth is as follows: spraying surface treatment agent I and surface treatment agent II on the surface of the glass fiber cloth in sequence, and drying to obtain the glass fiber cloth; The surface treatment agent I is composed of 0.5wt% of a silane coupling agent, 0.4wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 3 using a pH adjuster (acetic acid) before use; The surface treatment agent II is composed of 3 wt % of a silane coupling agent, 1.5 wt % of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 5 using a pH adjuster (acetic acid) before use.

[0037] The surfactants in surface treatment agent I and surface treatment agent II are both silicone nonionic surfactants (BYK-066N); The silane coupling agents in the surface treatment agent I and the surface treatment agent II are both composed of a mixture of γ-aminopropyltriethoxysilane and octyltriethoxysilane in a weight ratio of 1:0.3.

[0038] Application Example 12 The difference from Application Example 1 is that the weight ratio of the UV curing material to the glass fiber cloth used for trenchless pipeline repair is 0.5:1.

[0039] Application Example 13 The difference from Application Example 1 is that the weight ratio of the UV curing material to the glass fiber cloth used for trenchless pipeline repair is 0.7:1.

[0040] Application Example 14 The difference from Application Example 1 is that the weight ratio of the UV curing material to the glass fiber cloth used for trenchless pipeline repair is 0.3:1.

[0041] The glass fiber cloth is a surface-treated E-cR glass fiber cloth, and the surface treatment method of the E-cR glass fiber cloth is as follows: spraying surface treatment agent I and surface treatment agent II on the surface of the glass fiber cloth in sequence, and drying to obtain the glass fiber cloth; The surface treatment agent I is composed of 0.75wt% of a silane coupling agent, 0.5wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 3 using a pH adjuster before use; The surface treatment agent II is composed of 4 wt% of a silane coupling agent, 1.75 wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 5 using a pH adjuster before use.

[0042] Application Example 15 The difference from Application Example 1 is that the weight ratio of the UV curing material to the glass fiber cloth used for trenchless pipeline repair is 0.3:1.

[0043] The glass fiber cloth is a surface-treated E-cR glass fiber cloth, and the surface treatment method of the E-cR glass fiber cloth is as follows: spraying surface treatment agent I and surface treatment agent II on the surface of the glass fiber cloth in sequence, and drying to obtain the glass fiber cloth; The surface treatment agent I is composed of 1wt% of a silane coupling agent, 0.6wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 3 using a pH adjuster before use; The surface treatment agent II is composed of 5wt% of a silane coupling agent, 2wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 5 by a pH adjuster before use.

[0044] Application Example 16 The difference from Application Example 1 is that the silane coupling agent in both the surface treatment agent I and the surface treatment agent II is composed of a mixture of γ-aminopropyltriethoxysilane and octyltriethoxysilane in a weight ratio of 1:0.4.

[0045] Application Example 17 The difference from Application Example 1 is that the silane coupling agent in both surface treatment agent I and surface treatment agent II is composed of a mixture of γ-aminopropyltriethoxysilane and octyltriethoxysilane in a weight ratio of 1:0.5.

[0046] Comparative Example 1 The difference from Application Example 1 is that, in the preparation process of the UV curable material used, the unsaturated dibasic acid is only fumaric anhydride.

[0047] Comparative Example 2 The difference from Application Example 1 is that, during the preparation of the UV curable material, the unsaturated dibasic acid is only methacrylic anhydride.

[0048] Comparative Example 3 The difference from Application Example 1 is that in the preparation process of the UV curable material used, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to nadic anhydride is 0.3:1.

[0049] Comparative Example 4 The difference from Application Example 1 is that in the preparation process of the UV curable material used, the unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to nadic anhydride is 0.7:1.

[0050] Comparative Example 5 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the diol is neopentyl glycol.

[0051] Comparative Example 6 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the diol is 1,2-propylene glycol.

[0052] Comparative Example 7 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 1:1.

[0053] Comparative Example 8 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is 3:1.

[0054] Comparative Example 9 The difference from Application Example 1 is that, in the preparation process of the UV curing material used, the coupling agent is γ-aminopropyltriethoxysilane.

[0055] Comparative Example 10 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the coupling agent is octyltriethoxysilane.

[0056] Comparative Example 11 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane having a hydroxyl carbon atom number ≥ 6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane having a hydroxyl carbon atom number ≥ 6 is 1:1.

[0057] Comparative Example 12 The difference from Application Example 1 is that in the preparation process of the UV curing material used, the coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane having a hydroxyl carbon atom number ≥ 6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane having a hydroxyl carbon atom number ≥ 6 is 1:2.

[0058] The UV curable materials prepared in Examples 1-11 and Comparative Examples 1-12 were respectively taken as test objects, and their bending strength, bending modulus, tensile strength and bonding strength with steel sheets were measured and recorded in the following table.

[0059] Project Category Bending strength / MPa Flexural modulus / MPa Tensile strength / MPa Bonding strength with steel sheet / MPa Example 1 121.4 2512 81.2 5.3 Example 2 122.3 2524 82.6 5.7 Example 3 121.8 2518 81.2 5.4 Example 4 125.4 2529 83.1 5.9 Example 5 123.4 2522 82.6 5.6 Example 6 127.5 2533 83.9 6.2 Example 7 126.6 2531 83.3 6.0 Example 8 129.3 2536 84.4 6.4 Example 9 127.5 2529 83.7 6.1 Example 10 131.2 2539 84.7 6.6 Embodiment 11 129.7 2527 83.6 6.3 Comparative Example 1 107.5 2424 74.4 4.4 Comparative Example 2 105.7 2409 73.2 4.2 Comparative Example 3 111.5 2466 75.2 4.8 Comparative Example 4 112.2 2467 75.1 4.7 Comparative Example 5 105.2 2397 72.2 4.1 Comparative Example 6 103.2 2401 73.1 4.1 Comparative Example 7 109.4 2444 74.2 4.5 Comparative Example 8 110.2 2439 74.0 4.6 Comparative Example 9 110.2 2427 72.2 4.2 Comparative Example 10 109.8 2422 71.9 4.2 Comparative Example 11 114.2 2443 74.5 4.5 Comparative Example 12 115.1 2446 74.8 4.7 It can be seen from the data in the above table that the UV-curable materials prepared in Examples 1-11 of the present application have better bending strength, bending modulus, tensile strength and bonding strength with steel sheets than those in Comparative Examples 1-12.

[0060] Application Example 1-17 was used to perform trenchless repair on the pipeline. After the repair, the inner wall of the pipe was smooth and sealed. The repaired pipe had high strength and rigidity and could independently withstand internal and external pressures. The pipeline pressure test was 1.6MPa and the pressure was maintained for 1 hour without leakage, and the pressure was stable.

[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A UV curing material for trenchless pipeline repair. It is characterized in that The composition comprises the following components in parts by weight: Unsaturated polyester resin 50-80 parts; 10-40 parts of diluent; Photosensitizer 0.1-0.7 parts; Thickener 1-10 parts; Coupling agent 0.1-3 parts; Defoaming agent 0.1-2 parts; The unsaturated polyester resin is a linear polymer compound having an ester bond and an unsaturated double bond formed by polycondensation of an unsaturated dibasic acid and a diol; The unsaturated dibasic acid is a mixture of fumaric anhydride and methacrylic anhydride, wherein the weight ratio of fumaric anhydride to nadic anhydride is (0.4-0.6):1; The diol is a mixture of neopentyl glycol and 1,2-propylene glycol, wherein the weight ratio of neopentyl glycol to 1,2-propylene glycol is (1.5-2.5):1; The coupling agent is a mixture of γ-aminopropyltriethoxysilane and hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6, wherein the weight ratio of γ-aminopropyltriethoxysilane to hydrocarbon triethoxysilane with hydroxyl carbon atoms ≥6 is 1:(1.4-1.6).

2. The UV curing material for trenchless pipeline repair according to claim 1, It is characterized in that The unsaturated dibasic acid is composed of fumaric anhydride and nadic anhydride in a weight ratio of 0.5:1; The diol is composed of neopentyl glycol and 1,2-propylene glycol in a weight ratio of 2:

1.

3. The UV curing material for trenchless pipeline repair according to claim 1 or 2, It is characterized in that The preparation method of the unsaturated polyester resin comprises: in an inert atmosphere, carrying out a polycondensation reaction of a diol and an unsaturated dibasic acid under the catalytic action of a catalyst, and then adding a capping agent for capping to obtain the unsaturated polyester resin; Wherein, the weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the end-capping agent is 1:(1.4-1.6):(0.05-0.08):(0.1-0.2).

4. The UV curing material for trenchless pipeline repair according to claim 3, It is characterized in that The weight ratio of the diol, the unsaturated dibasic acid, the catalyst and the end-capping agent is 1:1.5:0.06:0.

15.

5. The UV curing material for trenchless pipeline repair according to claim 1, It is characterized in that The weight ratio of the γ-aminopropyltriethoxysilane to the hydrocarbon triethoxysilane having 6 or more hydroxyl carbon atoms is 1:1.

5.

6. The UV curing material for trenchless pipeline repair according to claim 5, It is characterized in that The hydrocarbyl triethoxysilane having 6 or more hydroxyl carbon atoms is octyl triethoxysilane.

7. A glass fiber cloth impregnated with the UV curing material for trenchless pipeline repair according to any one of claims 1 to 6.

8. The glass fiber cloth according to claim 7, It is characterized in that The weight ratio of the UV curing material for trenchless pipeline repair to the glass fiber cloth is (0.3-0.7):

1.

9. The glass fiber cloth according to claim 7 or 8, It is characterized in that The glass fiber cloth is a surface-treated E-cR glass fiber cloth, and the surface treatment method of the E-cR glass fiber cloth is: spraying surface treatment agent I and surface treatment agent II on the surface of the glass fiber cloth in sequence, and drying to obtain the glass fiber cloth; The surface treatment agent I is composed of 0.5-1wt% of a silane coupling agent, 0.4-0.6wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 3 using a pH adjuster before use; The surface treatment agent II is composed of 3-5wt% of a silane coupling agent, 1.5-2wt% of a surfactant and the balance of water, and the pH of the surface treatment agent I is adjusted to 5 with a pH adjuster before use.

10. The glass fiber cloth according to claim 9, It is characterized in that The surfactants in surface treatment agent I and surface treatment agent II are both silicone nonionic surfactants; The silane coupling agents in the surface treatment agent I and the surface treatment agent II are both composed of a mixture of gamma-aminopropyltriethoxysilane and octyltriethoxysilane in a weight ratio of 1:(0.3-0.5).

Citation Information

Cited By

  • Glass fiber prepreg tape and high-strength water supply pipe prepared from same