Composite precipitator for laterite-nickel ore wet refining and laterite-nickel ore wet refining method
By precipitating nickel and cobalt in acidic solution using a composite precipitant composed of magnesium oxide and sodium hydroxide, the problems of high consumption of sodium hydroxide and calcium oxide pollution in the prior art are solved, and high-efficiency and low-cost laterite nickel ore are achieved Wet refining process.
Patent Information
- Application Number
- CN202411084556.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
In the existing wet refining process of laterite nickel ore, sodium hydroxide, as a precipitant, has high consumption, high cost, difficult precipitate to settle and filtration, high moisture content of the filter cake, strong equipment corrosion and difficult tail water treatment, and oxidation Calcium precipitants lead to insoluble calcium sulfate contamination and pipeline blockage.
Using a composite precipitant composed of magnesium oxide and sodium hydroxide, the mass fraction of sodium hydroxide is between 0-99%, and the magnesium oxide content is greater than 88 wt.%, and magnesium oxide with high activity is formed through specific preparation methods and process conditions. Combined with sodium hydroxide, precipitating nickel and cobalt in acidic solution.
It realizes easy sedimentation and filtration of precipitates, low moisture content of filter cake, low cost, high production efficiency, reduced energy consumption and equipment corrosion, and improved the precipitation efficiency of nickel and cobalt.
Smart Images

Figure BDA0004984791190000051 
Figure BDA0004984791190000061 
Figure BDA0004984791190000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, in particular to a composite precipitant for hydrometallurgical refining of laterite nickel ore and a method for hydrometallurgical refining of laterite nickel ore. Background Art
[0002] In recent years, with the sharp increase in demand for power batteries in the new energy industry, the demand for nickel has increased rapidly. The wet refining of laterite nickel ore has become the main process for preparing nickel. In a high temperature and high pressure environment, sulfuric acid selectively leaches Ni, Co, Mg, Mn, etc. in laterite nickel ore. After neutralization, washing and impurity removal, the slurry is added with a precipitant to obtain the intermediate product MHP.
[0003] At present, the precipitant used in the nickel-cobalt precipitation process is mostly sodium hydroxide. Although the process of sodium hydroxide precipitation of nickel and cobalt is simple, it has major disadvantages: first, the consumption of sodium hydroxide is large (single ton of metal nickel needs to consume 4 tons of 50% liquid caustic soda), the storage area is very large, and the cost is high; second, sodium hydroxide has strong alkalinity, resulting in the formation of very fine or viscous precipitates, which are difficult to settle and filter, and are not conducive to the solid-liquid separation process. Therefore, flocculants are generally used in the concentration process, which increases the operating cost; third, due to the small particle size of the precipitate, the filter cake is also difficult to wash, and the filter cake has a high moisture content, which makes subsequent transportation and treatment difficult; fourth, sodium hydroxide has extremely strong alkalinity, resulting in all transportation, storage containers and process equipment being required to be resistant to strong alkali corrosion, and the investment cost is significantly increased; fifth, the sodium sulfate solution tail water generated after the reaction has high treatment cost and is difficult to handle.
[0004] Although calcium oxide or calcium hydroxide is used as a precipitant, the precipitant cost is low, but it will lead to the formation of insoluble calcium sulfate precipitate, which will remain in the nickel (cobalt) hydroxide product. Not only will it pollute the nickel / cobalt product, but the viscosity of calcium sulfate will also cause adhesion and blockage of the production process pipeline, making the production unable to run smoothly.
[0005] Therefore, it is imperative to develop new precipitants with cost advantages and high production process efficiency. Summary of the invention
[0006] Therefore, the technical problem to be solved by the present invention is to provide a composite precipitant for wet refining of laterite nickel ore, which has easy sedimentation and filtration of the precipitate and low moisture content of the filter cake, and a wet refining method of laterite nickel ore.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A composite precipitant for wet refining of laterite nickel ore comprises a mixture of magnesium oxide and sodium hydroxide, wherein the mass fraction of the sodium hydroxide in the composite precipitant is greater than 0 and less than or equal to 99%.
[0009] The mass fraction of sodium hydroxide in the composite precipitant for wet refining of laterite nickel ore is greater than 0 and less than or equal to 40%.
[0010] The above-mentioned composite precipitant for wet refining of laterite nickel ore, magnesium oxide (MgO) ≥88wt.%, loss on ignition ≤5wt.%, citric acid activity value is 10~100s, iodine absorption value is 60~150mgI 2 / gMgO, the active magnesium oxide accounts for 70-95wt.%, and the particle size D90≤100μm;
[0011] Preparation method of magnesium oxide: crush the dolomite to a particle size of 30 to 80 mm, calcine in a rotary kiln at 900 to 1100° C., and the kiln speed is 0.5 rpm to 2 rpm.
[0012] The above-mentioned composite precipitant for wet refining of laterite nickel ore, magnesium oxide (MgO) 90~95wt.%, l oss≤3wt.%, citric acid activity is 15~40s, iodine absorption value is 80~130mgI 2 / gMgO, active magnesium oxide accounts for 80-90wt.%, and particle size D90≤45μm.
[0013] The composite precipitant for wet refining of laterite nickel ore is prepared by adding magnesium oxide and sodium hydroxide into a polypropylene stirring tank, stirring and mixing them uniformly to obtain the composite precipitant.
[0014] The composite precipitant for wet refining of laterite nickel ore is prepared by first dissolving sodium hydroxide in water to prepare a saturated sodium hydroxide solution, then adding magnesium oxide to the saturated sodium hydroxide solution, evaporating the solution under stirring to obtain magnesium oxide adsorbing sodium hydroxide, and then impregnating the magnesium oxide adsorbing sodium hydroxide with a polyvinyl alcohol solution and drying the solution to obtain the composite precipitant.
[0015] In the composite precipitant for wet refining of laterite nickel ore, the volume ratio of the polyvinyl alcohol solution to the magnesium oxide adsorbing sodium hydroxide is 0.5-1:1, and the concentration of the polyvinyl alcohol solution is 5wt.%.
[0016] The wet refining method of laterite nickel ore comprises the following steps:
[0017] (1) adding the composite precipitant directly or after slurrying to the acidic solution to be refined, wherein the acidic solution to be refined is an acidic aqueous solution containing nickel, an acidic aqueous solution containing cobalt, or an acidic aqueous solution containing nickel and cobalt; the composite precipitant is the composite precipitant according to any one of claims 1 to 7;
[0018] (2) stirring to allow the composite precipitant to fully react with the acidic solution to be extracted;
[0019] (3) the mixed solution after the reaction is concentrated to obtain a clear liquid and a solid slurry;
[0020] (4) The solid slurry is filtered and washed with water to obtain a solid containing nickel hydroxide, cobalt hydroxide, or nickel hydroxide-cobalt hydroxide, thereby achieving the precipitation of nickel, cobalt, or nickel-cobalt.
[0021] In the above-mentioned laterite nickel ore wet refining method, in step (1): the pH of the acidic solution to be refined is 3 to 6, preferably 4.5 to 5.5.
[0022] In the above-mentioned wet refining method of laterite nickel ore, in step (1): the total amount of sodium hydroxide and magnesium oxide in the composite precipitant is 0.7 to 1.2 times, preferably 0.8 to 1.0 times, the total amount of nickel and cobalt in the acidic solution to be refined.
[0023] In the above-mentioned laterite nickel ore wet refining method, in step (1): the composite precipitant slurry concentration is greater than 0wt.% and less than or equal to 50wt.%, preferably 5% to 20%; the slurry is prepared by mechanical stirring, and the stirring rate is 50 to 300r / min, preferably 100 to 150r / min; the slurry preparation time is 5 to 200min, preferably 8 to 30min.
[0024] In the above-mentioned laterite nickel ore wet refining method, in step (2): the composite precipitant reacts with the acidic solution to be refined at a temperature of 25 to 95°C, preferably 50 to 65°C.
[0025] In the above-mentioned laterite nickel ore wet refining method, in step (2): the reaction time of the composite precipitant and the acidic solution to be refined is 3 to 8 hours, preferably 4 to 6 hours.
[0026] In the above-mentioned laterite nickel ore wet refining method, in step (2): the composite precipitant reacts with the acidic solution to be refined and is subjected to magnetic stirring or mechanical stirring at a stirring rate of 200 to 600 r / min.
[0027] In the above-mentioned laterite nickel ore wet refining method, in step (2): the pH at the end point of the reaction between the composite precipitant and the acidic solution to be refined is controlled at 7 to 9, preferably 7.5 to 8.2.
[0028] In the above-mentioned laterite nickel ore wet refining method, in step (3): the mixed solution after the reaction is concentrated by natural sedimentation or by adding 0.01 to 0.15 wt.% of PAM for sedimentation.
[0029] The chemical reactions involved in the present invention are mainly as follows:
[0030] The composite precipitant is added to the solution directly or after slurry mixing, and the magnesium oxide hydrolysis reaction:
[0031] MgO+H2 O→Mg(OH) 2 ↓
[0032] Ionization of composite precipitant in aqueous solution:
[0033] Mg(OH) 2 →Mg 2+ +2OH -
[0034] NaOH → Na + +OH -
[0035] The composite precipitant is added to the nickel (cobalt) acid solution, and the OH produced by the ionization of magnesium hydroxide and sodium hydroxide is - The ions combine with nickel (cobalt) ions in the solution to form nickel hydroxide (cobalt hydroxide precipitate):
[0036] Mg(OH) 2 +NiSO 4 →Ni(OH) 2 ↓+MgSO 4
[0037] 2NaOH+NiSO 4 →Ni(OH) 2 ↓+Na 2 SO 4
[0038] The technical solution of the present invention achieves the following beneficial technical effects:
[0039] (1) The OH ions per unit mole of magnesium oxide in the composite precipitant composed of magnesium oxide and sodium hydroxide in the present invention are - The amount of ions is the ionization of sodium hydroxide into OH - Therefore, when producing nickel hydroxide (cobalt hydroxide) precipitation, the unit consumption of the composite precipitant is lower and the precipitant cost is also lower.
[0040] (2) The alkalinity of the composite precipitant in the present invention is more "gentle" than the currently commonly used sodium hydroxide, and it is not easy to produce local "over-alkalinity" phenomenon during use. The generated nickel hydroxide (cobalt hydroxide) precipitate is easy to settle and filter, and the filter cake has a lower moisture content, which effectively solves the problem of difficulty in sedimentation and filtration when using sodium hydroxide as a precipitant. It also reduces the amount of flocculant used when the precipitate is settled, reduces the cost, and also improves the production efficiency, reducing the energy consumption of filter cake drying.
[0041] (3) The wet refining method of laterite nickel ore of the present invention adds a composite precipitant to a nickel (and cobalt) solution, and the nickel content of the obtained nickel hydroxide (cobalt hydroxide) precipitate is more than 40%, and the magnesium content is ≤2%. The composite precipitant has high efficiency in precipitating nickel (and cobalt), and the nickel content in the precipitate is relatively high.
[0042] (4) The composite precipitant and the wet refining method of laterite nickel ore of the present invention have simple process, low cost, easy process control, easy sedimentation and filtration of nickel hydroxide (and cobalt hydroxide) precipitate, which can significantly improve production efficiency and reduce energy consumption.
[0043] (5) The present invention obtains magnesium oxide with good activity by controlling the particle size, kiln temperature and kiln speed of magnesite entering the rotary kiln, and then obtains a composite precipitant by compounding the magnesium oxide with good activity with sodium hydroxide. The composite precipitant can reduce the water content of the filter cake of the liquid after aluminum and iron removal from laterite nickel ore, accelerate the sedimentation rate and filtration rate, and reduce the unit consumption of the composite precipitant. The magnesium oxide content with good activity increases its activity, so that the sedimentation rate and filtration rate increase with the increase of magnesium oxide content, and the water content of the filter cake decreases. At the same time, the presence of a small amount of sodium hydroxide in the composite precipitant will also increase the reaction rate.
[0044] (6) The reason for calculating the total amount of sodium hydroxide and magnesium oxide in the composite precipitant based on 0.8-1.0 times the total amount of nickel and cobalt in the solution in the beaker is that there is a lot of Mn in the solution to be refined. 2+ Yes, in order to prevent manganese from precipitating, the amount of precipitant added is controlled in production to control the precipitation rate of nickel and cobalt to about 80%. Although a sufficient amount of precipitant can completely precipitate nickel and cobalt, a large amount of manganese will appear in the precipitate, reducing the proportion of nickel and cobalt in the precipitate, which is not conducive to production. Although the solution containing nickel and cobalt is an acidic solution, a certain amount of composite precipitant is indeed required to neutralize the acidic solution, but the amount is very small and can be ignored. DETAILED DESCRIPTION
[0045] Example 1
[0046] PN-MH007 magnesium oxide and sodium hydroxide are selected to form a composite precipitant, wherein the purity of sodium hydroxide is 98%. The performance test of PN-MH007 magnesium oxide is shown in Table 1.
[0047] Table 1 PN-MH007 magnesium oxide performance indicators
[0048]
[0049]
[0050] PN-MH007 magnesium oxide and sodium hydroxide are loaded into a polypropylene mixing tank at a mass ratio of 8:2. A desiccant made of quicklime is fixed at the feed port and the discharge port of the mixing tank to prevent the composite precipitant from absorbing moisture. The composite precipitant is taken out after being mixed evenly in the mixing tank and sealed for later use.
[0051] The preparation method of PN-MH007 magnesium oxide is as follows: crushing magnesite to 30-60 mm, calcining in a rotary kiln at 900-1000° C., and the kiln speed is 0.5-1 rmp / min.
[0052] The solution was prepared according to the main element composition of the liquid after aluminum and iron removal from laterite nickel ore, and the pH of the solution was adjusted with sulfuric acid. The chemical composition of the nickel (cobalt) acidic solution is shown in Table 2.
[0053] Table 2 Solution preparation based on the main element composition of the aluminum-removed laterite nickel ore Unit: g / L
[0054] element Ni Co Mn Mg Ca <![CDATA[Fe 2+ ]]> Si pH content 2.20 0.30 2.56 10.02 0.40 0.15 0.01 4.9
[0055] A certain amount of prepared acidic solution containing nickel and cobalt is taken from a beaker and placed in a constant temperature water bath, the temperature is set to 55°C, and a mechanical stirrer is turned on to stir the solution in the beaker at a stirring rate of 350r / min.
[0056] The total amount of sodium hydroxide and magnesium oxide in the composite precipitant was calculated based on 0.8 times the total amount of nickel and cobalt in the solution in the beaker. Water was added to the composite precipitant and slurry was prepared at a concentration of 10wt.%. Mechanical stirring was used during slurry preparation at a speed of 120r / min and stirring was performed for 8 minutes to complete the slurry preparation process.
[0057] Slowly pour the composite precipitant slurry into the nickel and cobalt solution, react for 5 hours, and measure the pH of the solution in the beaker at the end of the reaction to be 7.7. After the reaction is completed, quickly take out the beaker, let it stand, and observe the solid sedimentation. After sedimentation (natural sedimentation or adding 0.01-0.15wt.% PAM for sedimentation), take out the supernatant, and vacuum filter the concentrated solid slurry. After filtration, spray water on the surface of the filter cake to wash the soluble salts entrained in the filter cake. Weigh the weight of the filter cake before and after drying to calculate the moisture content of the filter cake, and detect the chemical composition of the filter cake after drying.
[0058] As shown in Table 3, in this embodiment, the nickel precipitation rate reached 78.63%, the cobalt precipitation rate reached 80.00%, the Ni content in the nickel hydroxide precipitation reached 43.23%, the Mg content was 0.75%, the sedimentation rate was 0.09 cm / s, and the filtration rate reached 5.55 m 3 / (m 2 ×h), the sedimentation rate and filtration rate are much higher than those of sodium hydroxide under the same conditions, the filtration rate is good, and the unit consumption of composite precipitant is 737kg / t(Ni+Co) The unit consumption is much lower than that of sodium hydroxide, and the moisture content of the filter cake is also lower.
[0059] Table 3 Comparison of the effects of precipitants
[0060]
[0061] Note: 0.8 times of the composite precipitant means that the total amount of sodium hydroxide and magnesium oxide in the composite precipitant is 0.8 times the total amount of nickel and cobalt in the solution, and 0.8 times of sodium hydroxide means that the amount of sodium hydroxide is 0.8 times the total amount of nickel and cobalt in the solution.
[0062] Example 2
[0063] PN-MH007C magnesium oxide and sodium hydroxide are selected to form a composite precipitant, wherein the purity of sodium hydroxide is 98%. The performance test of PN-MH007C magnesium oxide is shown in Table 4.
[0064] Table 4 PN-MH007C magnesium oxide performance indicators
[0065]
[0066]
[0067] PN-MH007C magnesium oxide and sodium hydroxide are loaded into a polypropylene stirring tank in a mass ratio of 1:1. A desiccant made of quicklime is fixed at the feeding port and the discharging port of the stirring tank to prevent the composite precipitant from absorbing moisture. The composite precipitant is taken out after being mixed evenly in the stirring tank and sealed for later use.
[0068] The preparation method of PN-MH007C magnesium oxide is as follows: crushing magnesite to 40-70 mm, calcining in a rotary kiln at 950-1050° C., and the kiln speed is 1-1.5 rmp / min.
[0069] The solution was prepared according to the main element composition of the liquid after aluminum and iron removal from laterite nickel ore, and the pH of the solution was adjusted with sulfuric acid. The chemical composition of the nickel (cobalt) acidic solution is shown in Table 5.
[0070] Table 5 Solution preparation based on the main element composition of the aluminum-removed laterite nickel ore Unit: g / L
[0071] element Ni Co Mn Mg Ca <![CDATA[Fe 2+ ]]> Si pH content 2.20 0.30 2.56 10.02 0.40 0.15 0.01 5.1
[0072] A certain amount of prepared acidic solution containing nickel and cobalt is taken from a beaker and placed in a constant temperature water bath, the temperature is set to 65°C, and a mechanical stirrer is turned on to stir the solution in the beaker at a stirring rate of 500r / min.
[0073] The total amount of sodium hydroxide and magnesium oxide in the composite precipitant was calculated based on 0.85 times the total amount of nickel and cobalt in the solution in the beaker. Water was added to the composite precipitant and slurry was prepared at a concentration of 20wt.%. Mechanical stirring was used during slurry preparation at a speed of 150r / min and stirring was performed for 25 minutes to complete the slurry preparation process.
[0074] Slowly pour the composite precipitant slurry into the nickel (and cobalt) solution, react for 6 hours, and measure the pH of the solution in the beaker at the end of the reaction to be 7.8. After the reaction is completed, quickly take out the beaker, let it stand, and observe the solid sedimentation. After sedimentation (natural sedimentation or adding 0.01-0.15wt.% PAM for sedimentation), take out the supernatant, and vacuum filter the concentrated solid slurry. After filtration, spray water on the surface of the filter cake to wash the soluble salts entrained in the filter cake. Weigh the weight of the filter cake before and after drying to calculate the moisture content of the filter cake, and detect the chemical composition of the filter cake after drying.
[0075] As shown in Table 6, the nickel precipitation rate reached 84.09%, the cobalt precipitation rate reached 83.33%, the Ni content in the nickel hydroxide precipitation reached 46.33%, the Mg content was 0.37%, the sedimentation rate was 0.07 cm / s, and the filtration rate reached 2.29 m 3 / (m 2 ×h), the sedimentation rate and filtration rate are much higher than those of sodium hydroxide under the same conditions, the filtration rate is good, and the unit consumption of composite precipitant is 930kg / t (Ni+Co) The unit consumption is much lower than that of sodium hydroxide, and the moisture content of the filter cake is also lower.
[0076] Table 6 Comparison of the effects of precipitants
[0077]
[0078] Example 3
[0079] PN-MH007D magnesium oxide and sodium hydroxide were selected to form a composite precipitant, wherein the purity of sodium hydroxide was 98%. The performance test of PN-MH007D magnesium oxide is shown in Table 7.
[0080] Table 7 PN-MH007 magnesium oxide performance indicators
[0081]
[0082]
[0083] PN-MH007D magnesium oxide and sodium hydroxide are loaded into a polypropylene stirring tank at a mass ratio of 2:8. A desiccant made of quicklime is fixed at the feeding port and the discharging port of the stirring tank to prevent the composite precipitant from absorbing moisture. The composite precipitant is taken out after being mixed evenly in the stirring tank and sealed for later use.
[0084] The preparation method of PN-MH007D magnesium oxide is as follows: crushing magnesite to 50-80 mm, calcining in a rotary kiln at 1000-1100°C, and the kiln speed is 1.5-2 rpm.
[0085] The solution was prepared according to the main element composition of the liquid after aluminum and iron were removed from the laterite nickel ore, and the pH of the solution was adjusted with sulfuric acid. The chemical composition of the nickel (cobalt) acidic solution is shown in Table 8.
[0086] Table 8 Solution preparation based on the main element composition of the aluminum-removed laterite nickel ore Unit: g / L
[0087] element Ni Co Mn Mg Ca <![CDATA[Fe 2+ ]]> Si pH content 2.20 0.30 2.56 10.02 0.40 0.15 0.01 5.2
[0088] A certain amount of prepared acidic solution containing nickel and cobalt is taken from a beaker and placed in a constant temperature water bath, the temperature is set to 50°C, and a mechanical stirrer is turned on to stir the solution in the beaker at a stirring rate of 450r / min.
[0089] The total amount of sodium hydroxide and magnesium oxide in the composite precipitant was calculated based on 0.95 times the total amount of nickel and cobalt in the solution in the beaker. Water was added to the composite precipitant and slurry was prepared at a concentration of 15wt.%. Mechanical stirring was used during slurry preparation at a speed of 130r / min and stirring was performed for 20 minutes to complete the slurry preparation process.
[0090] Slowly pour the composite precipitant slurry into the nickel and cobalt solution, react for 6 hours, and measure the pH of the solution in the beaker at 7.9 at the end of the reaction. After the reaction is completed, quickly take out the beaker, let it stand, and observe the solid sedimentation. After sedimentation (natural sedimentation or adding 0.01-0.15wt.% PAM for sedimentation), take out the supernatant, and vacuum filter the concentrated solid slurry. After filtration, spray water on the surface of the filter cake to wash the soluble salts entrained in the filter cake. Weigh the weight of the filter cake before and after drying to calculate the moisture content of the filter cake, and detect the chemical composition of the filter cake after drying.
[0091] As shown in Table 9, in this embodiment, the nickel precipitation rate reached 84.54%, the cobalt precipitation rate reached 76.67%, the nickel hydroxide precipitation had a Ni content of 40.65%, a Mg content of 0.43%, a sedimentation rate of 0.03 cm / s, and a filtration rate of 0.81 m / s. 3 / (m 2 ×h), the sedimentation rate and filtration rate are much higher than those of sodium hydroxide under the same conditions, the filtration rate is good, and the unit consumption of composite precipitant is 1220kg / t (Ni+Co) The unit consumption is lower than that of sodium hydroxide, and the moisture content of the filter cake is also lower.
[0092] Table 9 Comparison of the effects of precipitants
[0093]
[0094] Example 4
[0095] PN-MH007 magnesium oxide and sodium hydroxide are selected to form a composite precipitant, wherein the purity of sodium hydroxide is 98%. The performance test of PN-MH007 magnesium oxide is shown in Table 10.
[0096] Table 10 PN-MH007 magnesium oxide performance indicators
[0097]
[0098]
[0099] The difference between this embodiment and embodiment 1 is that the method for preparing the composite precipitant using magnesium oxide and sodium hydroxide is different (the mass ratio of magnesium oxide to sodium hydroxide is still 8:2): sodium hydroxide is dissolved in water to prepare a saturated sodium hydroxide solution, and then magnesium oxide is added to the saturated sodium hydroxide solution, and evaporated to dryness under stirring to obtain magnesium oxide adsorbing sodium hydroxide, and the magnesium oxide adsorbing sodium hydroxide is impregnated with a polyvinyl alcohol solution at a volume ratio of 1:1 and then dried, and the concentration of the polyvinyl alcohol solution used is 5wt.%, to obtain a magnesium oxide-sodium hydroxide composite precipitant.
[0100] The solution was prepared according to the main element composition of the liquid after aluminum and iron were removed from the laterite nickel ore, and the pH of the solution was adjusted with sulfuric acid. The chemical composition of the nickel (cobalt) acidic solution is shown in Table 11.
[0101] Table 11 Solution preparation based on the main element composition of the aluminum-removed laterite nickel ore Unit: g / L
[0102] element Ni Co Mn Mg Ca <![CDATA[Fe 2+ ]]> Si pH content 2.20 0.30 2.56 10.02 0.40 0.15 0.01 4.9
[0103] A certain amount of prepared acidic solution containing nickel and cobalt is taken from a beaker and placed in a constant temperature water bath, the temperature is set to 55°C, and a mechanical stirrer is turned on to stir the solution in the beaker at a stirring rate of 350r / min.
[0104] The total amount of sodium hydroxide and magnesium oxide in the composite precipitant was calculated based on 0.8 times the total amount of nickel and cobalt in the solution in the beaker. Water was added to the composite precipitant and slurry was prepared at a concentration of 10wt.%. Mechanical stirring was used during slurry preparation at a speed of 120r / min and stirring was performed for 8 minutes to complete the slurry preparation process.
[0105] Slowly pour the composite precipitant slurry into the nickel and cobalt solution, react for 5 hours, and measure the pH of the solution in the beaker at the end of the reaction to be 7.6. After the reaction is completed, quickly take out the beaker, let it stand, and observe the solid sedimentation. After sedimentation (natural sedimentation or adding 0.01-0.15wt.% PAM for sedimentation), take out the supernatant, and vacuum filter the concentrated solid slurry. After filtration, spray water on the surface of the filter cake to wash the soluble salts entrained in the filter cake. Weigh the weight of the filter cake before and after drying to calculate the moisture content of the filter cake, and detect the chemical composition of the filter cake after drying.
[0106] As shown in Table 12, in this embodiment, the nickel precipitation rate reached 78.18%, the cobalt precipitation rate reached 76.67%, the Ni content in the nickel hydroxide precipitation reached 43.18%, the Mg content was 0.72%, the sedimentation rate was 0.101 cm / s, and the filtration rate reached 6.28 m 3 / (m 2 ×h), the sedimentation rate and filtration rate are much higher than those of sodium hydroxide under the same conditions, the filtration rate is good, and the unit consumption of composite precipitant is 741kg / t (Ni+Co) The unit consumption is much lower than that of sodium hydroxide, and the moisture content of the filter cake is also lower.
[0107] Table 12 Comparison of the effects of precipitants
[0108]
[0109] Sodium hydroxide adsorbs polyvinyl alcohol and causes polyvinyl alcohol to crystallize, thereby sealing the sodium hydroxide in the micropores of the magnesium oxide particles, so that the magnesium oxide-sodium hydroxide composite precipitant can slowly release sodium hydroxide during the reaction, increase the particle size of the precipitate, increase the sedimentation and filtration speed, and reduce the moisture content of the filter cake.
[0110] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A composite precipitant for wet refining of laterite nickel ore, characterized in that: The composite precipitant is a mixture consisting of magnesium oxide and sodium hydroxide, wherein the mass fraction of the sodium hydroxide in the composite precipitant is greater than 0 and less than or equal to 99%.
2. The composite precipitant for wet refining of laterite nickel ore according to claim 1, characterized in that: The mass fraction of sodium hydroxide in the composite precipitant is greater than 0 and less than or equal to 40%.
3. The composite precipitant for wet refining of laterite nickel ore according to claim 1, characterized in that: Magnesium oxide (MgO) ≥88wt.%, loss on ignition≤5wt.%, citric acid activity value is 10~100s, iodine absorption value is 60~150mgI2 / gMgO, active magnesium oxide accounts for 70~95wt.%, particle size D90≤100μm; Preparation method of magnesium oxide: crush the dolomite to a particle size of 30 to 80 mm, calcine in a rotary kiln at 900 to 1100° C., and the kiln speed is 0.5 rpm to 2 rpm.
4. The composite precipitant for wet refining of laterite nickel ore according to claim 3, characterized in that: Magnesium oxide (MgO) At 90-95wt.%, loss≤3wt.%, citric acid activity is 15-40s, iodine absorption value is 80-130mgI2 / gMgO, active magnesium oxide accounts for 80-90wt.%, particle size D90≤45μm.
5. A composite precipitant for wet refining of laterite nickel ore according to any one of claims 1 to 4, characterized in that: Add magnesium oxide and sodium hydroxide into a polypropylene stirring tank, stir and mix them evenly to obtain a composite precipitant.
6. A composite precipitant for wet refining of laterite nickel ore according to any one of claims 1 to 4, characterized in that: Firstly, sodium hydroxide is dissolved in water to prepare a saturated sodium hydroxide solution, and then magnesium oxide is added to the saturated sodium hydroxide solution, and evaporated to dryness under stirring to obtain magnesium oxide adsorbing sodium hydroxide, and the magnesium oxide adsorbing sodium hydroxide is impregnated with a polyvinyl alcohol solution and then dried to obtain a composite precipitant.
7. The composite precipitant for wet refining of laterite nickel ore according to claim 6, characterized in that: The volume ratio of the polyvinyl alcohol solution to the magnesium oxide adsorbing sodium hydroxide is 0.5-1:1, and the concentration of the polyvinyl alcohol solution is 5wt.%.
8. A wet refining method for laterite nickel ore, characterized in that: The steps include: (1) adding the composite precipitant directly or after slurrying to the acidic solution to be refined, wherein the acidic solution to be refined is an acidic aqueous solution containing nickel, an acidic aqueous solution containing cobalt, or an acidic aqueous solution containing nickel and cobalt; the composite precipitant is the composite precipitant according to any one of claims 1 to 7; (2) stirring to allow the composite precipitant to fully react with the acidic solution to be extracted; (3) the mixed solution after the reaction is concentrated to obtain a clear liquid and a solid slurry; (4) The solid slurry is filtered and washed with water to obtain a solid containing nickel hydroxide, cobalt hydroxide, or nickel hydroxide-cobalt hydroxide, thereby achieving the precipitation of nickel, cobalt, or nickel-cobalt.
9. The wet refining method of laterite nickel ore according to claim 8, characterized in that: In step (1): the pH of the acidic solution to be extracted is 3 to 6, preferably 4.5 to 5.
5.
10. The wet refining method of laterite nickel ore according to claim 8, characterized in that: In step (1): the total amount of sodium hydroxide and magnesium oxide in the composite precipitant is 0.7 to 1.2 times, preferably 0.8 to 1.0 times, the total amount of nickel and cobalt in the acidic solution to be refined; in step (1): the slurry concentration of the composite precipitant is greater than 0wt.% and less than or equal to 50wt.%, preferably 5% to 20%; the slurry is mechanically stirred, the stirring rate is 50 to 300r / min, preferably 100 to 150r / min; the slurry adjustment time is 5 to 200min, preferably 8 to 30min; in step (2): the composite precipitant reacts with the acidic solution to be refined, The temperature is 25 to 95° C., preferably 50 to 65° C.; in step (2): the reaction time of the composite precipitant and the acidic solution to be refined is 3 to 8 hours, preferably 4 to 6 hours; in step (2): the composite precipitant and the acidic solution to be refined are reacted by magnetic stirring or mechanical stirring, and the stirring rate is 200 to 600 r / min; in step (2): the pH of the composite precipitant and the acidic solution to be refined is controlled at 7 to 9, preferably 7.5 to 8.2 at the end point of the reaction; in step (3): the concentration of the mixed solution after the reaction is natural sedimentation or the addition of 0.01 to 0.15 wt.% PAM for sedimentation.
Citation Information
Patent Citations
Application of caustic calcined magnesite powder to recovery of nickel and cobalt
CN102851504A
High-activity magnesite powder and manufacturing method thereof and method for reclaiming nickel cobalt from laterite nickel ores
CN102874852A
Method for recycling cobalt from cobaltous sulfate solution
CN108998682A
Nickel precipitation method for laterite-nickel ore leachate without bringing in impurities
CN111422928A
System and process for extracting nickel and cobalt from laterite nickel ore through two-stage pressurization
CN113564383A
Cited By
Method for preparing MHP through cyclic utilization of manganese precipitation post-solution and application of MHP
CN119491112A
Method for preparing MHP by recycling post-manganese precipitation liquid and application thereof
CN119491112B
Method for precipitating nickel and cobalt by activating magnesium oxide with alkaline solution and cobalt nickel hydroxide product
CN120719141A